Created by Glazy Admin 2015-07-16 06:59:40, updated 2015-09-20 05:23:32

Theoretical Material

Type: Feldspar

Weight: 0.0000
Formula Weight: 524.3500
LOI: 0.0000
Thermal Expansion: 0.0000
Oxide SiO2 Al2O3 Na2O
% Analysis 68.74 19.44 11.82
Formula 5.999 1.000 1.000

Map to your favorite soda feldspar, or use one of the analyses below.
Analyses:
Cooper & Royle: (Harrison Mayer Ltd. 36.0.021)
% 7.48 Na2O 2.78 K2O 1.88 CaO 19.00 Al2O3 67.90 SiO2 0.11 Fe2O3 0.29 LOI
Tichane (AG):
% 7.0 Na2O 4.5 K2O 1.8 CaO 19.7 Al2O3 66.8 SiO2
Parmelee: (typical)
% 9.37 Na2O 0.41 K2O 2.06 CaO 21.76 Al2O3 66.22 SiO2 0.04 Fe2O3 0.16 LOI

Hazards

09/2016 Note: This is a new feature. If there is no safety information below, then that material's data has not yet been added. Some materials only have GHS ratings, while others only have HMIS ratings. Warnings differ between systems and countries. Glazy does not take any responsibility for accuracy of linked SDS information. Contact your ceramics supplier for safety information for your specific materials.

This material's safety information has not yet been added to Glazy.

Recipes using this material

Name Amount of Soda Feldspar (Theoretical) Temp. Atmospheres Surface Transparency Si:Al R20:RO Author
Lime green 18 Δ5½ - 6 Oxidation
Glossy Transparent 10.31 0.22 : 0.78 Daniel Spruyt
G14:5 18 Δ6 - 9 Oxidation
Glossy Transparent 10.31 0.22 : 0.78 Cecilia Ekengren
Folk Art Guild White- 3134 Sn6.5/Zr6.5 (variation) 18 Δ5 - 6 Oxidation
Glossy 6.97 0.26 : 0.74 Allathea Joniec
Triin's Tenmoku Gold 18.4 Δ6 - 7 Oxidation
Glossy Translucent 10.48 0.39 : 0.61 Triin Lehismets
SA Orange Shino 33 Δ9 - 11 Reduction
Salt & Soda
Wood
Satin Opaque 4.65 0.95 : 0.05 Anglian Potters
Emmanuel Cooper Wide-Firing Clear Base Glaze + Variations 38 Δ5 - 7 Oxidation
Reduction
Semi-glossy Translucent 11.39 0.2 : 0.8 Jayne Bunting
Bright Purple 35 Δ5 - 7 Oxidation
Satin-matte Semi-opaque 9.1 0.21 : 0.79 Jayne Bunting
Shino C Pot Camp standard 35 Δ9 - 10 Oxidation
Reduction
Wood
Glossy Translucent 4.26 0.97 : 0.03 Ruth Gillett
Shino B smooth satin or gloss 70 Δ9 - 10 Oxidation
Reduction
Wood
Glossy Translucent 5.44 0.97 : 0.03 Ruth Gillett
Shino A shiny 35 Δ9 - 10 Oxidation
Reduction
Wood
Glossy Semi-opaque 4.19 0.98 : 0.02 Ruth Gillett
Peter Legstrump Fischer Rutile Blue Glaze 44   Translucent 9.59 0.29 : 0.71 Ceramic Recipes
FM Matte Ferreira 2 20 Δ5½ - 6 Oxidation
Satin-matte Semi-opaque 10.16 0.12 : 0.88 Clara Giorello
Selsor Chun SiC, RIO 0.5/1/1.5/2 34 Δ5 Oxidation
Glossy Semi-opaque 15.12 0.26 : 0.74 Clara Giorello
Harris Average 25.2 Δ4 - 5½ Oxidation
Satin Opaque 4.61 0.16 : 0.84 Clara Giorello
Harris Average Rutile 25.2 Δ5½ Oxidation
Satin Opaque 4.62 0.16 : 0.84 Clara Giorello
Selsor Chun, RIO 0.5/1/1.5/2 34 Δ5 Reduction
15.12 0.26 : 0.74 Clara Giorello
Waxy white Shino 40 Δ7 - 8 Oxidation
Satin-matte Translucent 4.14 0.96 : 0.04 Made in Mokum
Folk Art Guild White- 3134/Sn13 18 Δ5 - 6 Oxidation
Semi-glossy Opaque 6.71 0.26 : 0.74 Clara Giorello
Astor#23 Base 26 Δ5 - 6 Oxidation
Satin Translucent 8.58 0.38 : 0.62 Clara Giorello
Harris #7 Rutile Variation 21.38 Δ5 - 6 Oxidation
Reduction
Glossy Opaque 8.5 0.16 : 0.84 Clara Giorello
FM Matte Ferreira 3 20 Δ5½ Oxidation
Satin-matte Semi-opaque 10.16 0.12 : 0.88 Clara Giorello
FM Matte Ferreira 1 20 Δ5½ Oxidation
Satin-matte Semi-opaque 10.16 0.12 : 0.88 Clara Giorello
FM Matte White 20 Δ5½ Oxidation
Satin-matte Semi-opaque 10.16 0.12 : 0.88 Clara Giorello
Cushing's Satin 20 Δ9 - 10 Reduction
Satin Opaque 10.63 0.17 : 0.83 IU Southeast Ceramics
Harris #32 31.5 Δ5 Oxidation
Matte Opaque 13.88 0.16 : 0.84 Clara Giorello
Harris Tenmoku Red (variation) 18.6 Δ5 Oxidation
Matte Opaque 12.68 0.16 : 0.84 Clara Giorello
Harris #27 Tam (Ball Clay) 29.47 Δ5 Oxidation
Matte Opaque 11.91 0.16 : 0.84 Clara Giorello
Harris #26 K (Kaolin) 33.6 Δ5 Oxidation
Semi-glossy Opaque 7.97 0.16 : 0.84 Clara Giorello
Harris #23 Tam (Ball Clay) 23.7 Δ5 Oxidation
Matte Opaque 13.45 0.16 : 0.84 Clara Giorello
Harris #22 Tam (Ball Clay) 27.45 Δ5 Oxidation
Matte Opaque 10.47 0.16 : 0.84 Clara Giorello
Harris #18 Tam (Ball Clay) 22.05 Δ5 Oxidation
Matte Opaque 11.87 0.16 : 0.84 Clara Giorello
Harris #17 Tam (Ball Clay) 25.42 Δ5 Oxidation
Smooth Matte Opaque 9.36 0.16 : 0.84 Clara Giorello
Harris #16 Tam (Ball Clay) 28.8 Δ5 Oxidation
Satin Opaque 7.39 0.16 : 0.84 Clara Giorello
Harris #12 Tam (Ball Clay) 23.4 Δ5 Oxidation
Satin Opaque 8.49 0.16 : 0.84 Clara Giorello
Harris #11 Tam (Ball Clay) 26.4 Δ5 Oxidation
Semi-glossy Opaque 6.79 0.16 : 0.84 Clara Giorello
Harris #8 K (Kaolin) 18.75 Δ5 Oxidation
Semi-glossy Opaque 6.54 0.16 : 0.84 Clara Giorello
Harris #7 Tam (Ball Clay) 21.38 Δ5 - 6 Oxidation
Reduction
Glossy Opaque 7.79 0.17 : 0.83 Clara Giorello
Harris #7 K (Kaolin) 21.38 Δ5 - 6 Oxidation
Glossy Opaque 5.47 0.16 : 0.84 Clara Giorello
Harris #6 Tam (Ball Clay) 24 Δ5 Oxidation
Glossy Opaque 6.31 0.17 : 0.83 Clara Giorello
Harris #3 K (kaolin) 17.1 Δ5 Oxidation
Satin Opaque 5.77 0.16 : 0.84 Clara Giorello