Materials with Percentage Analysis

Ingredient Type Parent SiO2 Al2O3 B2O3 MgO CaO SrO BaO ZnO Li2O K2O Na2O P2O5 Fe2O3 TiO2 MnO MnO2 F PbO LOI
A.P. Green, AP Green Fire Clay Clay Fire clay (Theoretical) 52.24 31.14   0.35 0.35         1.00     2.01 1.91         11.00
Ajax Glomax kaolin Clay Kaolin, China Clay (Theoretical) 53.16 44.40               0.41 0.30   0.42 0.94         0.38
Ajax P kaolin Clay Kaolin, China Clay (Theoretical) 45.39 38.12   0.30 0.25         0.04     0.48 1.97         13.45
Alajo kiln ash Ash 8.52 1.55   5.33 41.30         1.03 0.44 3.68 1.27           36.88
Albany slip Clay 57.83 14.63   2.71 5.81         3.20 0.80   5.21 0.40         9.41
Alberta Slip, Archie Bray Slip Clay 54.54 15.48   3.97 6.01         3.57 2.24 0.10 4.58 0.31         9.20
Alkaline Frit Frit 66.88 6.02 2.89   5.64         3.45 15.12                
Alkaline leadless frit Frit 56.10 4.00 8.00   6.40     10.90   2.00 12.30                
Alumina Alumina   100.00                                  
Alumina Hydrate Alumina   65.39                                 34.61
Ingredient Type Parent SiO2 Al2O3 B2O3 MgO CaO SrO BaO ZnO Li2O K2O Na2O P2O5 Fe2O3 TiO2 MnO MnO2 F PbO LOI
Aluminum sulfate Alumina   29.80                                 70.20
Amblygonite Flux   24.50             10.10     48.00             17.40
Anhydrous Borax Flux     69.18               30.82                
Antimony oxide Colorant                                      
Applewood ash Ash 2.06     4.20 54.15         9.01 1.45 3.43             25.70
Arsenic oxide Colorant                                      
Avery kaolin Clay Kaolin, China Clay (Theoretical) 46.75 37.54               0.90 0.20   0.70 0.10         13.80
Bainbridge Feldspar Feldspar Soda Feldspar (Theoretical) 68.60 19.29     0.99         1.39 9.23               0.50
Ball Clay (Theoretical) Clay Theoretical 59.06 25.02   0.30 0.30         0.90 0.40   1.02 1.00         12.00
Ball Clay Bell Dark Clay Ball Clay (Theoretical) 58.45 26.59   0.40 0.20         0.69 0.19   1.08 2.08         10.30
Ingredient Type Parent SiO2 Al2O3 B2O3 MgO CaO SrO BaO ZnO Li2O K2O Na2O P2O5 Fe2O3 TiO2 MnO MnO2 F PbO LOI
Bamboo ash Ash 86.40       0.30         4.80     0.40           8.10
Bandy Black Clay Ball Clay (Theoretical) 61.09 24.53   0.12 0.09         1.70 0.36 0.07 1.00 1.29 0.02       9.74
Bandy Tan Clay Ball Clay (Theoretical) 61.44 24.47   0.58 0.32         1.65 0.36 0.03 1.19 1.27 0.02       8.67
Barium Carbonate Flux             77.66                       22.34
Barium chloride Flux             73.60                       26.40
Barium chromate Colorant             60.50                       9.50
Barium selenite Colorant             58.00                        
Barium sulfate Flux             65.70                        
Barley straw ash Ash 57.00     3.00 8.00         22.00 5.00 5.00              
Barnard Clay, Blackbird Clay Clay 46.99 7.60   0.70 0.60         1.10 0.60   33.90 0.20         8.31
Ingredient Type Parent SiO2 Al2O3 B2O3 MgO CaO SrO BaO ZnO Li2O K2O Na2O P2O5 Fe2O3 TiO2 MnO MnO2 F PbO LOI
Basalt Feldspar 52.00 14.00   6.40 9.30         1.20 3.20 0.40 12.80 1.00          
Beech ash Ash 3.01     8.20 42.00         24.29 8.34 6.20 0.62   4.52        
Bell Feldspar Feldspar Potash Feldspar (Theoretical) 68.28 17.87     0.40         10.08 3.09   0.08           0.21
Bentolite L Clay Montmorillonite Clay (Theoretical) 72.70 13.70   2.70 2.00         0.10 0.20   0.70 0.20         7.70
Bentonite Clay Montmorillonite Clay (Theoretical) 59.33 20.12   2.01 1.01         1.01 3.02   3.51           10.00
Birch ash Ash 11.50     14.30 29.60         22.60 9.00 7.90 1.30   0.40       3.40
Bismuth oxide Colorant                                      
Bismuth subnitrate Colorant                                      
Black Iron Oxide, BIO Colorant                         65.93           8.00
Black stain Colorant                                      
Ingredient Type Parent SiO2 Al2O3 B2O3 MgO CaO SrO BaO ZnO Li2O K2O Na2O P2O5 Fe2O3 TiO2 MnO MnO2 F PbO LOI
Bonding Clay Clay 54.76 29.43   0.30 0.20         1.70 0.20   1.70 1.60         10.10
Bone Ash, Calcium Phosphate Opacifier         55.82             42.39             1.79
Boraq Flux 13.48 2.80 29.96 2.30 21.77         0.60 3.60   0.20           25.30
Borax Flux     36.53               16.26               47.21
Boric Acid Flux     56.40                               43.60
Borocalcite Flux 4.90 0.08 44.00 0.80 26.30         0.50     0.02           22.30
Buckingham feldspar Feldspar Potash Feldspar (Theoretical) 66.89 18.00   0.10 0.20         11.59 2.99               0.22
Burnt sienna Colorant 20.02 2.91     1.07               76.00            
Burnt umber Colorant 19.90 6.83   1.65 3.76               59.42   8.45        
C & C ball clay Clay Ball Clay (Theoretical) 59.83 26.29   0.20 0.10         0.41 0.20 0.02 0.92 1.64         10.40
Ingredient Type Parent SiO2 Al2O3 B2O3 MgO CaO SrO BaO ZnO Li2O K2O Na2O P2O5 Fe2O3 TiO2 MnO MnO2 F PbO LOI
C W-5 clay Clay 48.80 35.70   0.20 0.30         1.00 1.00   1.60 1.80         13.20
C-6 Soda Feldspar Feldspar Soda Feldspar (Theoretical) 68.39 18.47   0.06 0.70         5.19 6.89   0.06           0.24
Cadmium carbonate Colorant                                      
Cadmium sulfide Colorant                                      
Cadycal Flux 0.49 0.10 46.80 0.24 25.62 0.03       0.01 0.10   0.05           26.57
Calcined Kaolin Clay 54.10 45.90                                  
Calcined Talc, Magnesium Silicate 63.38     31.87                              
Calcium Borate Flux     55.39   44.61                            
Calcium borate frit Frit 17.85 4.88 50.02 0.20 26.59         0.46                  
Calcium chloride Flux                                      
Ingredient Type Parent SiO2 Al2O3 B2O3 MgO CaO SrO BaO ZnO Li2O K2O Na2O P2O5 Fe2O3 TiO2 MnO MnO2 F PbO LOI
Calcium phosphate Flux         54.24             45.76              
Calcium sulfate Flux         41.20                           58.80
Calcium zirconium silicate Opacifier 25.10       23.43                            
Calvert Clay Clay 57.79 23.80   0.80 0.30         2.00 0.41   5.71 1.21         7.98
Carbondale Red Fire Clay Clay Fire clay (Theoretical) 56.09 19.19   0.64 0.56 0.02 0.14     0.51 0.60 0.08 12.02 1.04 0.03       9.04
Carolina Stone Feldspar 73.00 16.40     0.60         4.50 4.40   0.05           1.10
Cedar ash Ash 24.28 0.52   6.00 44.20         4.30 3.70 10.60 1.01   0.30       5.09
Cedar Height Stoneware Clay 66.62 22.06   0.11 0.57           0.50   1.70 0.31         8.13
Cerium oxide Flux                                      
Cherry ash Ash 33.50     12.00 41.00             10.00 3.50            
Ingredient Type Parent SiO2 Al2O3 B2O3 MgO CaO SrO BaO ZnO Li2O K2O Na2O P2O5 Fe2O3 TiO2 MnO MnO2 F PbO LOI
Chesterfield Feldspar Feldspar Potash Feldspar (Theoretical) 70.75 16.34     0.30         8.50 3.75   0.07           0.29
Chrome Oxide, Chromium Oxide Colorant                                      
Chromium sulfate Colorant                                     82.90
Clay (Theoretical) Clay Theoretical 46.23 37.77   0.10 0.18         0.34 0.06 0.24 0.80 0.37         13.91
Clinchfield #202 Feldspar Potash Feldspar (Theoretical) 68.53 16.78     0.34         10.85 2.50               1.00
Clinchfield #303 Feldspar Potash Feldspar (Theoretical) 67.87 18.22     0.50         7.91 5.51                
CMC Miscellaneous                                      
Coal ash Ash 42.90 22.74   1.73 6.61               12.33 13.70          
Cobalt Carbonate Colorant                                     37.00
Cobalt chloride Colorant                                     68.50
Ingredient Type Parent SiO2 Al2O3 B2O3 MgO CaO SrO BaO ZnO Li2O K2O Na2O P2O5 Fe2O3 TiO2 MnO MnO2 F PbO LOI
Cobalt nitrate Colorant                                     74.30
Cobalt Oxide, Black Cobalt Oxide Colorant                                     6.65
Cobalt sulfate Colorant                                     73.30
Colemanite Flux     50.80   27.30                           21.90
Common ash Ash 30.99 8.91   3.30 22.42         3.91 2.33 1.91 3.04   1.26       21.44
Copper Carbonate Colorant                                     35.62
Copper chloride Colorant                                     53.30
Copper Oxide, Black Copper Oxide Colorant                                      
Copper Sulfate Colorant                                     68.10
Cornwall Stone Feldspar 73.78 16.33   0.14 1.81         4.30 3.30   0.19 0.15          
Ingredient Type Parent SiO2 Al2O3 B2O3 MgO CaO SrO BaO ZnO Li2O K2O Na2O P2O5 Fe2O3 TiO2 MnO MnO2 F PbO LOI
Cornwall stone - DF Feldspar 79.58 12.01     0.20         3.80 3.90   0.06           0.45
Cornwall stone - Hard White Feldspar 72.00 18.20   0.15 0.35         5.50 0.25 0.10 0.13 0.05         3.50
Cornwall stone - Purple Feldspar 72.80 15.80   0.12 1.90         3.70 3.60 0.38 0.18 0.07         1.25
Crocus martis Colorant                         44.14           20.88
Cryolite Flux   24.30                 44.30           54.30    
Custer Feldspar Feldspar Potash Feldspar (Theoretical) 68.50 17.00     0.30         10.00 3.00   0.10           0.30
Custer Feldspar (1989) Feldspar Potash Feldspar (Theoretical) 68.64 17.39     0.30         10.36 3.02               0.30
Custer Feldspar (2000-2012 Ron Roy) Feldspar Potash Feldspar (Theoretical) 72.40 15.27   0.07 0.27         7.52 3.21 0.20 0.21           0.65
Custer Feldspar (pre-2000) Feldspar Potash Feldspar (Theoretical) 68.70 17.25   0.05 0.18         10.06 3.04 0.31 0.12           0.66
Darvan Miscellaneous                                      
Ingredient Type Parent SiO2 Al2O3 B2O3 MgO CaO SrO BaO ZnO Li2O K2O Na2O P2O5 Fe2O3 TiO2 MnO MnO2 F PbO LOI
Del Monte feldspar Feldspar 73.40 16.50   0.20 0.20         4.30 4.70   0.15 0.02         0.45
Desert plant ash Ash       0.50 21.10         5.50 28.00 1.80              
Dextrine Miscellaneous                                      
Diamond Kaolin Clay Kaolin, China Clay (Theoretical) 45.81 38.07   0.10 0.15         0.18 0.08   0.70 1.41         13.50
Dolomite Flux       21.91 30.48                           47.61
Elder ash Ash 14.00     16.00 38.00         17.00 2.00 13.00              
Epidote Feldspar 12.00 3.00     8.00               3.00            
EPK, EP Kaolin, Edgar Plastic Clay Kaolin, China Clay (Theoretical) 45.73 37.36   0.10 0.18         0.35 0.07 0.26 0.76 0.38         14.81
Epsom salts, Magnesium Sulfate Flux       16.35                             83.65
Eureka Feldspar Feldspar Potash Feldspar (Theoretical) 69.75 17.06     0.01         9.38 3.49   0.10           0.20
Ingredient Type Parent SiO2 Al2O3 B2O3 MgO CaO SrO BaO ZnO Li2O K2O Na2O P2O5 Fe2O3 TiO2 MnO MnO2 F PbO LOI
Eureka Feldspar #703 Feldspar Soda Feldspar (Theoretical) 73.58 15.52     0.16         6.16 4.58                
F-20 Feldspar Feldspar Soda Feldspar (Theoretical) 68.53 18.95     1.41         4.13 6.85   0.06           0.08
Feldspar Feldspar 64.76 18.32               16.92                  
Feldspar FFF Feldspar 66.99 19.05   0.10 0.30         8.42 5.01   0.12            
Fern ash Ash 55.02 19.32   7.44 8.59         4.81 0.56 0.92 1.67 0.30 1.36        
Ferro Feldspar #10 Feldspar 71.77 15.27               10.26 2.70                
Ferro Frit 3249 Frit 42.10 13.30 28.90 12.20 3.50                            
Ferro Frit CC-279-3, CC-279 Frit 52.50 7.50 17.50 0.50 7.50 2.50   0.50 2.50 5.00 7.50           2.50    
Fire clay (Theoretical) Clay Theoretical 57.46 28.53   0.23 0.09         1.00 0.17   1.25 1.99         9.28
Fluorspar Flux         59.60                       40.40    
Ingredient Type Parent SiO2 Al2O3 B2O3 MgO CaO SrO BaO ZnO Li2O K2O Na2O P2O5 Fe2O3 TiO2 MnO MnO2 F PbO LOI
Formaldehyde Miscellaneous                                      
Foundry Hill Creme Clay Ball Clay (Theoretical) 66.68 20.65   0.50 0.50         0.71 0.55 0.09 1.61 0.50         8.20
Fremington clay Clay 59.68 20.11   3.97 4.87         3.98 0.44   6.01 0.94          
Frit 1362W Frit 72.98 1.40   3.87 8.45           13.30                
Frit 1455W Frit 56.45 10.78 9.81   12.29           10.67                
Frit 1460W Frit 46.20 12.63 16.24             6.87 18.07                
Frit 1461W Frit 49.40   35.01               15.58                
Frit 1462W Frit 37.50 7.58 42.77   12.15                            
Frit 1463W Frit 59.33 10.07 17.87   12.73                            
Frit 210507 Frit 50.70 5.74 3.92   6.31         15.90 17.43                
Ingredient Type Parent SiO2 Al2O3 B2O3 MgO CaO SrO BaO ZnO Li2O K2O Na2O P2O5 Fe2O3 TiO2 MnO MnO2 F PbO LOI
Frit 210701 Frit 48.55 9.67 17.96   12.13         4.65 7.05                
Frit 210702 Frit 50.23 14.49 18.64   11.95         2.83 1.86                
Frit 210703 Frit 36.69 4.98 11.48   5.48     35.28   2.30 3.78                
Frit 210704 Frit 52.48 6.75 16.71 0.33 16.02         0.78 6.93                
Frit 211701 Frit 55.34 6.24 13.23 0.78 6.14     1.05   2.12 4.79                
Frit 213702 Frit 53.61 11.46 13.27 0.49 6.03         5.07 2.42             7.64  
Frit 3002 Frit 48.55 9.67 17.96   12.13         4.65 7.05                
Frit 3003 Frit 60.78   16.25   10.91           12.06                
Frit 3005 Frit 54.56 7.97 12.81 1.00 5.15     1.10     5.71                
Frit 3006 Frit 51.42 5.25 19.59 0.16 12.89         1.12 9.58                
Ingredient Type Parent SiO2 Al2O3 B2O3 MgO CaO SrO BaO ZnO Li2O K2O Na2O P2O5 Fe2O3 TiO2 MnO MnO2 F PbO LOI
Frit 3110 Frit 66.88 6.02 2.89   5.64         3.45 15.12                
Frit 3124 Frit 55.30 9.90 13.77   14.07         0.68 6.28                
Frit 3134 Frit 46.51   23.09   20.13           10.28                
Frit 3185 Frit 54.10   38.20               7.70                
Frit 3191 Frit 48.30   27.97   11.27           12.46                
Frit 3195 Frit 48.35 11.98 22.62   11.36           5.69                
Frit 3226 Ferro Frit 52.50 1.00 36.30   2.90           7.30                
Frit 3240 Frit 5.68 0.13 1.44   1.27   1.14 2.27   0.08 0.65           0.27    
Frit 3247 Frit 41.61 5.30         53.09                        
Frit 3269 Frit 43.10 19.42 15.28   0.08     1.17   11.01 9.93                
Ingredient Type Parent SiO2 Al2O3 B2O3 MgO CaO SrO BaO ZnO Li2O K2O Na2O P2O5 Fe2O3 TiO2 MnO MnO2 F PbO LOI
Frit 3278 Frit 56.31   21.73   6.85           15.11                
Frit 3288 Frit 50.36 4.97 18.82   16.91         0.42 8.52                
Frit 3289 Frit 33.21 6.17 9.68       47.12       3.82                
Frit 3292 Frit 61.50 10.80 5.70 0.70 10.60 4.20     0.40 3.10 3.00                
Frit 3293 Frit 76.40 5.90   0.80 0.20           16.70                
Frit 3300 Frit 38.80 9.20   0.40 8.80   6.20 10.50   3.20 0.70             22.20  
Frit 3304 Frit 40.50 4.00                 1.10             54.40  
Frit 3403 Frit 28.10 2.30     0.10         1.40 0.30             67.80  
Frit 3417 Frit 43.60 3.00 12.60   4.50         1.90 1.50             30.50  
Frit 3419 Frit 19.90   14.50               6.40             59.20  
Ingredient Type Parent SiO2 Al2O3 B2O3 MgO CaO SrO BaO ZnO Li2O K2O Na2O P2O5 Fe2O3 TiO2 MnO MnO2 F PbO LOI
Frit 3465 Frit 52.50   20.20   6.50           14.40             6.40  
Frit 3467 Frit 56.50 9.10 4.50 0.60 8.00         1.70 2.40             17.20  
Frit 3470 Frit 27.70 5.80 8.50   5.60     9.00     2.20             41.20  
Frit 3481 Frit 49.90 7.00 6.20   9.90         1.20 3.10             22.80  
Frit 3489 Frit 26.80       5.60                         67.60  
Frit 3493 Frit 44.70 3.10 12.90   4.60         1.90 1.50             31.30  
Frit 3496 Frit 49.70 4.90 4.30   4.20         1.40 2.40             33.10  
Frit 3565 Frit 54.00 5.60 7.80   9.90         3.00 1.60             16.00  
Frit 3576 Frit 40.40 3.50 13.70   4.80           3.80             33.00  
Frit 36.2.191 Frit 32.20 2.80                               65.00  
Ingredient Type Parent SiO2 Al2O3 B2O3 MgO CaO SrO BaO ZnO Li2O K2O Na2O P2O5 Fe2O3 TiO2 MnO MnO2 F PbO LOI
Frit 36.2.192 Frit 49.00 7.50 18.30   15.00         1.20 9.00                
Frit 36.2.193 Frit 56.10 4.00 8.00   6.40     10.90   2.00 12.30                
Frit 36.2.194 Frit 54.40 5.70 10.60         5.20   0.20 7.20                
Frit 36.2.195 Frit 51.00 6.70 10.20   7.20       0.30 1.30 5.20             18.00  
Frit 3819 Frit 41.60 18.64 16.77   0.25     1.19   9.85 11.70                
Frit 3831 Frit 42.70 10.60     12.20   17.90     12.00 4.60                
Frit 5301 Frit 42.45 19.60 13.82   2.14         8.22 13.77                
Frit CC-257-2 Frit 46.60 9.20   0.31 5.50 0.57 33.80     0.79 1.00     2.20          
Frit CC298-2 Frit 31.00 7.00 28.00 3.50 21.00         3.50 6.00                
Frit F-15 Fusion Frit 61.79 5.95 24.58             5.21 2.47                
Ingredient Type Parent SiO2 Al2O3 B2O3 MgO CaO SrO BaO ZnO Li2O K2O Na2O P2O5 Fe2O3 TiO2 MnO MnO2 F PbO LOI
Frit F-245 Fusion Frit 49.23 1.43 39.63   2.63           7.08                
Frit F-280 Fusion Frit 49.17 12.94 15.59   11.88         9.84 0.56                
frit F-38 Fusion Frit 44.78 5.99 14.65   3.29 24.43         4.79                
Frit F-496 Fusion Frit 71.60 2.59 17.70             2.39 5.71                
Frit F-524 Fusion Frit 56.90 9.50 12.00   7.30 7.61 2.00     2.59 2.10                
Frit F-71 Fusion Frit 58.44 5.78 5.92   5.82         3.56 20.48                
Frit F-79 Fusion Frit 47.56 13.71 27.55   4.02 1.55     0.22 1.68 3.70                
Frit F12 Fusion Frit 45.00 0.80 23.80   20.00           10.40                
Frit F18 Fusion Frit 59.50 6.80 8.90   11.80 8.00       2.40 2.60                
Frit P-1733 Frit 40.70   30.20   4.20     15.50     9.40                
Ingredient Type Parent SiO2 Al2O3 B2O3 MgO CaO SrO BaO ZnO Li2O K2O Na2O P2O5 Fe2O3 TiO2 MnO MnO2 F PbO LOI
Frit P-1836 Frit 48.82 10.00 2.98   5.50   14.18 13.84   1.41 3.27                
Frit P-1855 Frit 21.09 0.27 7.94 0.03 0.03     0.30 0.09 0.46 0.09                
Frit P-25 Frit 49.69 12.09 16.90   0.51     0.71   5.41 14.70                
Frit P-283 Frit 76.50 5.90   0.70 0.30           16.60                
Frit P-311 Frit 54.31 10.01 14.41   14.09         0.69 6.49                
Frit P-404 Frit 42.60 10.80     12.18   17.80     12.00 4.61                
Frit P-54 Frit 46.30   23.30   20.00           10.40                
Frit P-626 Frit 49.20 5.40 12.40       27.39       5.60                
Frit P-64 Frit 39.80 1.00 9.70   8.90   8.10 15.30   0.40 4.80                
Frit P-830 Frit 56.30   21.60   7.20           14.90                
Ingredient Type Parent SiO2 Al2O3 B2O3 MgO CaO SrO BaO ZnO Li2O K2O Na2O P2O5 Fe2O3 TiO2 MnO MnO2 F PbO LOI
Frit P-926 Pemco Frit 50.48 5.02 18.71   17.01         0.29 8.49                
Frit P2241 Frit 32.50 2.60                               64.90  
Frit P2242 Frit 28.50                         2.90       68.70  
Frit P2244 Frit 17.74 4.78 50.60   27.10                            
Frit P2245 Frit 48.70 9.00 13.60 0.03 8.86         8.66 11.15                
Frit P2246 Frit 48.90 7.47 18.66 0.05 15.02         1.29 8.66                
Frit P2247 Frit 62.00 9.37 14.84 0.15 7.31         2.73 3.60                
Frit P2248 Frit 55.00 4.50 14.70   7.40     2.30     6.00                
Frit P2250 Frit 50.70 5.74 3.92   6.31         15.90 17.43                
Frit P2251 Frit 58.53 9.70 18.08   5.75         1.20 6.73                
Ingredient Type Parent SiO2 Al2O3 B2O3 MgO CaO SrO BaO ZnO Li2O K2O Na2O P2O5 Fe2O3 TiO2 MnO MnO2 F PbO LOI
Frit P2252 Frit 65.80 6.70 15.35 2.20 3.68     0.90     5.44                
Frit Pb Frit 35.00                                 65.00  
Frit Pb-1038 Frit 35.90 5.00 5.00         7.60   0.30 2.70             43.50  
Frit Pb-1114 Frit 40.70 3.50 11.10   9.80         1.40 1.90             31.60  
Frit Pb-197 Frit 53.00 7.40 6.50   5.90     9.50   2.40 4.00             11.30  
Frit Pb-1V48 Frit 47.00 3.10 14.80   0.80         1.50 9.50             17.20  
Frit Pb-316 Frit 31.70 7.00                               61.30  
Frit Pb-349 Frit 53.80 6.20 8.00   10.40         2.70 1.80             17.10  
Frit Pb-41 Frit 13.40   9.00         5.40                   72.20  
Frit Pb-63 Frit 43.00 3.40 12.60   4.50           3.60             30.50  
Ingredient Type Parent SiO2 Al2O3 B2O3 MgO CaO SrO BaO ZnO Li2O K2O Na2O P2O5 Fe2O3 TiO2 MnO MnO2 F PbO LOI
Frit Pb-716 Frit 26.80       5.60                         67.60  
Frit Pb-723 Frit 24.90 2.40                 1.50             71.20  
Frit Pb-740 Frit 20.00 2.00           20.00     1.20             56.80  
Frit Pb-742 Frit 43.50 3.40 13.00   4.50           3.60             31.00  
Frit Pb-83 Frit 20.00   14.40               6.40             59.20  
Frit Pb-943 Frit 52.70   20.30   6.30         5.30 9.00             6.30  
Frit, Fusion 134 Frit 60.50 11.50 6.00   11.00 4.50     0.40 1.20 4.90                
Frit, Fusion 367 Frit 53.80   38.40               7.80                
Frit, Fusion 75 Frit 70.00 3.70 2.50   6.40         2.10 15.30                
Frit, Hommel 14 Frit 46.35   23.28   19.98           10.39                
Ingredient Type Parent SiO2 Al2O3 B2O3 MgO CaO SrO BaO ZnO Li2O K2O Na2O P2O5 Fe2O3 TiO2 MnO MnO2 F PbO LOI
Frit, Hommel 25 Frit 49.70 12.10 16.90   0.50     0.70   5.40 14.70                
Frit, Johnson Matthey 169 Frit 35.92 0.49 27.51 0.01 2.49 0.15 7.73 5.96     19.61     0.02          
Frit, Johnson Matthey 623 Frit 34.88 0.29 28.38   2.33   9.09 5.85     19.19                
Fuller's earth Clay 66.82 19.75   2.26 3.38               7.79            
Fusion Frit F-493 Frit 51.80 6.30 13.20           11.00 6.00 11.70                
G-200 EU Feldspar Feldspar Potash Feldspar (Theoretical) 68.50 17.00   0.08 0.50         11.00 2.10   0.10 0.03         0.50
G-200 Feldspar Feldspar Potash Feldspar (Theoretical) 66.44 18.54   0.05 0.80         10.82 3.11   0.09           0.15
G-40 feldspar Feldspar Potash Feldspar (Theoretical) 67.56 18.00     0.80         10.40 3.00   0.07           0.16
G200 HP Feldspar, G200HP Feldspar Potash Feldspar (Theoretical) 66.00 18.30     0.30         14.20 0.90   0.09           0.15
Galena Flux                                   93.30 6.70
Ingredient Type Parent SiO2 Al2O3 B2O3 MgO CaO SrO BaO ZnO Li2O K2O Na2O P2O5 Fe2O3 TiO2 MnO MnO2 F PbO LOI
Georgia Kaolin Clay Kaolin, China Clay (Theoretical) 52.74 44.46   0.16 0.28         0.16 0.05   0.51 1.65          
Gerstley Borate Flux Theoretical 14.80 1.00 26.80 3.50 19.40         0.40 4.00 0.10 0.40 0.10         29.50
Gillespie Borate Flux Gerstley Borate 11.80 1.70 24.49 3.90 22.99 0.45         3.77               30.90
Glass, Powdered Glass Flux 71.47 1.14   3.28 10.12         0.09 13.68   0.23            
Glomax Clay 53.15 44.40     0.05         0.41 0.30   0.42 0.94         0.38
Godfrey feldspar Feldspar 74.31 17.07     2.86           5.54               1.50
Gold chloride Colorant                                      
Goldart Clay 55.26 28.83   0.40 0.20         1.90 0.20   1.40 1.80         10.00
Granite Feldspar 70.18 13.49     1.99         4.11 3.48   1.57           0.84
Granular ilmenite Colorant                           52.64          
Ingredient Type Parent SiO2 Al2O3 B2O3 MgO CaO SrO BaO ZnO Li2O K2O Na2O P2O5 Fe2O3 TiO2 MnO MnO2 F PbO LOI
Granular manganese Colorant                               86.90     13.10
Granular rutile Colorant                         9.90 90.00         0.10
Grass ash Ash 66.51 11.29   6.69 15.52                            
Green nickel oxide Colorant                                      
Grog Clay                                      
Grog, fine Miscellaneous                                      
Grog, med Miscellaneous                                      
Grolleg Kaolin Clay Kaolin, China Clay (Theoretical) 47.92 36.94   0.30 0.10         1.90 0.10   0.70 0.03         12.01
Gum arabic Miscellaneous                                      
Gypsum Flux                                      
Ingredient Type Parent SiO2 Al2O3 B2O3 MgO CaO SrO BaO ZnO Li2O K2O Na2O P2O5 Fe2O3 TiO2 MnO MnO2 F PbO LOI
Hamilton kaolin Clay Kaolin, China Clay (Theoretical) 45.81 38.07   0.10 0.15         0.18 0.08   0.70 1.41         13.50
Hardwood ash Flux 0.67     15.85 21.51         33.44 2.30 16.34 0.58   2.60       6.71
Hawthorne Bond Clay Fire clay (Theoretical) 51.06 35.24   0.70 0.30         1.30 0.10   1.40 1.90         8.00
Hazel ash Ash 10.00     15.00 26.00         35.00 10.00 4.00              
Hearth ash Ash 14.08 3.69   5.44 35.90         1.49 0.55 2.14 0.94   0.14        
Heather ash Ash 41.00     10.00 21.00         12.00 9.00 5.00 2.00            
Helmer Kaolin, Helmar Kaolin Clay 46.54 36.42   0.26 0.49         0.54 0.08   1.32 1.14         13.22
Hyplas 71 Ball clay Clay Ball Clay (Theoretical) 70.50 18.75   0.30 0.10         1.80 0.30   0.80 1.60         5.30
Ilmenite Colorant                           52.64          
Imacco 800 Clay 49.65 31.53   0.50 0.04         0.51 0.51   6.44           10.81
Ingredient Type Parent SiO2 Al2O3 B2O3 MgO CaO SrO BaO ZnO Li2O K2O Na2O P2O5 Fe2O3 TiO2 MnO MnO2 F PbO LOI
Imco 800 Fireclay Clay Fire clay (Theoretical) 53.20 28.60   0.67 0.18         1.69 0.15   4.51 1.27         7.30
Imco Borate Flux 22.99 0.44 26.59 1.96 20.92 2.18       1.53 3.27   0.33           19.80
Iron carbonate Colorant                         68.90           31.10
Iron chloride Colorant                         29.50           70.50
Iron chromate Colorant                         46.50           9.30
Iron oxide Colorant                         95.00           5.00
Iron spangles Colorant                         66.17            
Iron sulfate, Ferrous sulfate Colorant                         28.70           71.30
Isu-wood ash Ash 34.60 4.38   5.99 47.71         2.51 0.06 3.93 0.49   0.33        
Ivy ash Ash 12.00     8.00 25.00         26.00 20.00 6.00 3.00            
Ingredient Type Parent SiO2 Al2O3 B2O3 MgO CaO SrO BaO ZnO Li2O K2O Na2O P2O5 Fe2O3 TiO2 MnO MnO2 F PbO LOI
Jackson Ball Clay Clay Ball Clay (Theoretical) 54.32 30.10   0.30 0.20         0.90 0.20   0.80 2.49         10.70
Jordan Fire Clay Clay Fire clay (Theoretical) 67.24 20.18   0.50 0.20         1.99 0.20   1.71 1.20         6.78
K-200 Feldspar Feldspar 68.07 17.86     0.18         10.14 3.36   0.08           0.31
K&T Special Ball Clay Clay Ball Clay (Theoretical) 53.30 27.40   0.50 0.30         0.90 0.20   1.10 1.50         14.80
Kaolin, China Clay (Theoretical) Clay Theoretical 47.29 40.21                                 12.50
Kaopaque 20 Kaolin Clay Kaolin, China Clay (Theoretical) 46.34 40.29   0.03 0.22         0.08 0.03   0.33 0.68         12.00
Kentucky #1 Ball Clay, Kentucky No. 1 Clay Ball Clay (Theoretical) 57.36 29.02   0.39 0.10         0.79 0.39   1.18 0.98         9.80
Kentucky #12 Ball Clay Clay Ball Clay (Theoretical) 51.24 27.97   0.30 0.40         1.00 0.20   0.90 1.70         16.30
Kentucky #6 Clay Ball Clay (Theoretical) 58.73 28.06   0.10           0.90 0.20   0.80 1.21         10.00
Kentucky ball clay Clay Ball Clay (Theoretical) 55.20 27.90   0.40 0.30         1.00 0.30   1.10 1.20         12.60
Ingredient Type Parent SiO2 Al2O3 B2O3 MgO CaO SrO BaO ZnO Li2O K2O Na2O P2O5 Fe2O3 TiO2 MnO MnO2 F PbO LOI
Kentucky OM #4 Ball Clay, OM-4, OM4, Old Mine 4 Clay Ball Clay (Theoretical) 55.20 27.90   0.40 0.30         1.00 0.30   1.10 1.20         12.60
Kentucky Special Ball Clay Clay Ball Clay (Theoretical) 54.43 27.47   0.50 0.50         1.10 0.20   1.20 1.30         13.30
Kentucky Stone Clay Ball Clay (Theoretical) 68.05 19.72   0.49 0.20         1.18 0.20   1.78 1.28         7.10
Keystone feldspar Feldspar Potash Feldspar (Theoretical) 64.61 19.86               13.34 2.19                
Kingman Feldspar Feldspar 66.18 18.72     0.10         12.01 2.80   0.11           0.08
Kingsley kaolin Clay Kaolin, China Clay (Theoretical) 44.79 38.39   0.04 0.90         0.14 0.11   0.39 1.64         13.60
Kona A-3 Feldspar Feldspar Potash Feldspar (Theoretical) 71.63 16.30     0.40         7.51 4.00   0.07           0.09
Kona F-4 feldspar, Kona F4 Feldspar Soda Feldspar (Theoretical) 66.74 19.58   0.05 1.70         4.80 6.89   0.04           0.20
Kyanite Clay 37.08 62.92                                  
Laguna Borate Flux Gerstley Borate 18.68 8.09 27.47 2.30 18.88         1.40 4.00   0.10 0.10         19.00
Ingredient Type Parent SiO2 Al2O3 B2O3 MgO CaO SrO BaO ZnO Li2O K2O Na2O P2O5 Fe2O3 TiO2 MnO MnO2 F PbO LOI
Larch wood ash Ash 11.00 1.00   8.00 27.00         21.00 9.00 8.00 4.00   11.00        
Lead antimonate Colorant                                   67.40 3.20
Lead Bisilicate Frit Flux 35.00                                 65.00  
Lead Carbonate, White lead Flux                                   86.51 13.49
Lead chloride Flux                                   80.30 19.70
Lead chromate Colorant                                   69.10 7.40
Lead dioxide Flux                                   93.30 6.70
Lead monosilicate Flux 15.00                                 85.00  
Lead orthosilicate Flux                                      
Lead sesquisilicate Flux 28.76                                 71.24  
Ingredient Type Parent SiO2 Al2O3 B2O3 MgO CaO SrO BaO ZnO Li2O K2O Na2O P2O5 Fe2O3 TiO2 MnO MnO2 F PbO LOI
Lead sulfate Flux                                   73.60 26.40
Lead trioxide Flux                                   87.50 12.50
Lepidolite Feldspar 47.92 27.03             3.01 7.33                 14.70
Lime feldspar - theoretical Feldspar 69.52 19.66     10.82                            
Limestone Flux 5.03 0.81   7.94 42.83         0.33 0.05 0.04 0.54 0.06         42.36
Lincoln Fire Clay Clay Fire clay (Theoretical) 52.15 32.59   0.60 0.20         0.75 0.30   2.21           11.20
Litharge Flux                                   100.00  
Lithium Carbonate Flux                 40.74                   59.26
Lithospar Feldspar 69.36 21.69             2.00 2.91 4.04                
Lizella Red Clay 63.70 19.60   0.78 0.70         1.40 0.85   3.60 1.00         8.50
Ingredient Type Parent SiO2 Al2O3 B2O3 MgO CaO SrO BaO ZnO Li2O K2O Na2O P2O5 Fe2O3 TiO2 MnO MnO2 F PbO LOI
Lunday kaolin Clay Kaolin, China Clay (Theoretical) 47.35 36.34               1.30 0.30   1.00 0.10         13.60
M&D Ball Clay Clay Ball Clay (Theoretical) 57.46 27.33   0.50 0.50         0.50     2.31 1.31         10.09
M23 Ball Clay Clay Ball Clay (Theoretical) 58.78 27.74   0.20 0.20         0.60 0.08   1.00 1.50         9.90
Macaloid Clay Montmorillonite Clay (Theoretical) 53.35 0.82   22.72 6.68       1.23   3.19   0.31           11.70
Madoc H spar Feldspar Potash Feldspar (Theoretical) 67.24 18.54     0.49         10.05 3.68                
Magnesium carbonate, Magnesite Flux       47.80                             52.20
Magnesium chloride Flux       19.80                             80.20
Magnesium zirconium silicate Opacifier 28.94     19.41                              
Mahavir Potash Feldspar Feldspar Potash Feldspar (Theoretical) 67.00 17.50   0.15 0.15         11.50 3.00   0.08           0.50
Mahogany ash Ash 51.51 3.81   4.39 9.49         9.49 10.98 2.08 4.53           3.72
Ingredient Type Parent SiO2 Al2O3 B2O3 MgO CaO SrO BaO ZnO Li2O K2O Na2O P2O5 Fe2O3 TiO2 MnO MnO2 F PbO LOI
Maine feldspar Feldspar Potash Feldspar (Theoretical) 70.95 17.30   0.11 0.20         8.12 2.82               0.50
Manganese Carbonate Colorant                             61.62       38.38
Manganese Dioxide Colorant                               86.90     13.10
Maple ash Ash 13.80 0.90   12.05 27.50         6.20 6.04 8.10 2.50   0.50       22.41
Mason 6600 black stain Colorant                                      
Mason stain Colorant                                      
McNamee Kaolin Clay Kaolin, China Clay (Theoretical) 44.46 39.34   0.05 0.06         0.31 0.04   0.33 1.20         13.99
Meadow hay ash Ash 29.57     5.00 11.56         25.67 7.00 6.20 1.00           14.00
Meerschaum Flux 69.10     30.90                              
Mineral flux no. 4 Feldspar 80.18 11.12     1.64         2.20 4.16   0.14           0.23
Ingredient Type Parent SiO2 Al2O3 B2O3 MgO CaO SrO BaO ZnO Li2O K2O Na2O P2O5 Fe2O3 TiO2 MnO MnO2 F PbO LOI
Minpro #4 Feldspar Feldspar Soda Feldspar (Theoretical) 69.49 18.54     0.83         5.55 5.59                
Minspar 200 Feldspar Feldspar Soda Feldspar (Theoretical) 68.91 18.58     1.51         4.12 6.53   0.06           0.30
Missouri Fire Clay Clay Fire clay (Theoretical) 52.24 31.14   0.35 0.35         1.00     2.01 1.91         11.00
Mixed wood ash Flux 19.84 1.44   6.64 20.84         22.07 6.82 13.63 8.72            
Molochite Clay 54.40 41.92   0.31 0.07         2.01 0.10   1.12 0.07          
Molybdenum oxide Colorant                                      
Monmouth Fire Clay Clay Fire clay (Theoretical) 50.96 45.01   0.30 0.11         0.55 0.01   2.21 0.84          
Monmouth stoneware clay Clay 56.80 28.50   0.30 0.30         0.30 0.30               12.20
Montmorillonite Clay (Theoretical) Clay Theoretical 43.77 18.57     1.02           1.13                
Mullite Clay 41.00 57.00               0.20 0.20   1.00 0.60          
Ingredient Type Parent SiO2 Al2O3 B2O3 MgO CaO SrO BaO ZnO Li2O K2O Na2O P2O5 Fe2O3 TiO2 MnO MnO2 F PbO LOI
Murrays Borate Flux 27.80 0.50 36.10   24.90           5.70               5.00
Narco fire clay Clay Fire clay (Theoretical) 52.53 31.10   0.60 0.13         2.19 0.30   1.84 1.74         9.58
NC-4 Feldspar Feldspar Soda Feldspar (Theoretical) 68.49 18.94   0.05 1.41         4.12 6.83   0.07           0.09
Nepheline Syenite Norwegian Feldspar Nepheline Syenite, Neph Sye (Theoretical) 58.47 23.19               8.57 7.56   0.20           2.00
Nepheline Syenite, Neph Sye (Theoretical) Feldspar Theoretical 60.70 23.30   0.10 0.70         4.60 9.80   0.10           0.70
New Zealand Halloysite, Kaolin Clay Kaolin, China Clay (Theoretical) 50.42 35.50                     0.22 0.06         13.80
Newman Red Clay Clay 64.68 18.04   1.46 0.30           0.25   6.05 2.22         7.30
Nickel Carbonate Colorant                                     37.07
Nickel Oxide, Black Nickel Oxide Colorant                                      
Niter Colorant                   46.60                 53.40
Ingredient Type Parent SiO2 Al2O3 B2O3 MgO CaO SrO BaO ZnO Li2O K2O Na2O P2O5 Fe2O3 TiO2 MnO MnO2 F PbO LOI
Oak ash Ash 15.30 0.10   12.00 30.00         14.00 9.12 13.10 2.40   0.10       3.88
Oat straw ash Ash 49.00     4.00 7.00         30.00 4.00 5.00 1.00            
Ocmulgee Clay 53.86 21.82   0.79 0.37         1.29 0.36   6.40 1.20 0.23       8.90
Oldenwalder Clay Clay 68.74 16.41   1.68 0.28         4.39 0.40 0.23   1.15          
Opax Opacifier 6.48 0.91                 1.11                
Oxford Feldspar Feldspar Potash Feldspar (Theoretical) 70.69 17.32     0.39         8.06 3.27   0.09           0.18
P-609 Frit 53.02 12.19 9.37 1.98 5.94 13.16     0.76 1.55 2.03                
Parks Ball Clay Clay Ball Clay (Theoretical) 58.90 26.80   0.10 0.30         0.10 0.20   0.80 1.60         11.20
PBX Fire Clay Clay Fire clay (Theoretical) 56.63 38.52   0.35 0.36               1.75 1.51         0.88
Pearl Ash, Potassium Carbonate Flux                   68.00                 32.00
Ingredient Type Parent SiO2 Al2O3 B2O3 MgO CaO SrO BaO ZnO Li2O K2O Na2O P2O5 Fe2O3 TiO2 MnO MnO2 F PbO LOI
Peerless #2 kaolin Clay Kaolin, China Clay (Theoretical) 44.60 39.50   0.10 0.10         0.50     0.50 1.40         13.30
Peerless kaolin Clay Kaolin, China Clay (Theoretical) 45.05 39.90   0.07 0.05         0.52 0.04   0.46 1.41         12.50
Petalite Feldspar 78.49 16.65             4.87                    
Pine Lake Clay 58.60 27.30   0.10 0.30         0.60 0.20   1.50 1.90         9.50
Pine wood ash Ash 2.00     8.21 41.09         10.96 0.77 4.67 0.07   2.54       29.69
Pioneer Kaolin Clay Kaolin, China Clay (Theoretical) 45.47 38.36   0.10 0.20           0.10   0.40 1.40         13.96
Plaster of Paris Flux         38.60                           61.40
Plastic Vitrox, PV Clay Feldspar 76.50 12.70   0.50 1.00         5.00 0.90   0.50 0.10         2.80
Portland cement Flux 22.50 7.50   2.00 62.50               2.50           2.00
Potash Feldspar (Theoretical) Feldspar Theoretical 64.76 18.32               16.92                  
Ingredient Type Parent SiO2 Al2O3 B2O3 MgO CaO SrO BaO ZnO Li2O K2O Na2O P2O5 Fe2O3 TiO2 MnO MnO2 F PbO LOI
Potassium chromate Colorant                   30.40                 20.60
Potassium dichromate Colorant                   32.00                 16.30
Potassium permanganate Colorant                   29.80         44.90       25.30
Potassium silicofluoride Flux 27.30                 42.80             51.70    
Potato tuber ash Ash 37.01 15.82   2.46 1.05         36.32   7.34              
PotteryCrafts Frit P2960 Frit 63.46 8.51 17.62 2.20 3.70     3.20 1.10 0.20                  
Praseodymium oxide Colorant                                      
Putnam kaolin Clay Kaolin, China Clay (Theoretical) 47.00 37.80   0.20 0.10         0.20 0.20   0.80 0.20         13.50
Pyrax Miscellaneous 78.21 16.08   0.10 0.10         1.81 0.30   0.20 0.10         3.10
Pyrophyllite Clay 67.70 28.30                                 4.00
Ingredient Type Parent SiO2 Al2O3 B2O3 MgO CaO SrO BaO ZnO Li2O K2O Na2O P2O5 Fe2O3 TiO2 MnO MnO2 F PbO LOI
Pyrotrol Clay 77.08 18.92               0.20 0.20   0.40 0.40         2.80
Ranger Red Clay Clay                                      
Ravenscrag Slip Clay Clay (Theoretical) 56.70 15.40   2.50 8.50         4.10 0.50   1.10 0.40         8.70
Raw sienna Colorant 23.13 13.07                     52.20           11.60
Raw umber Colorant 15.19 3.36   2.36 5.75               58.51   14.82        
Red clay Clay 64.95 15.51   1.59 0.26         4.15 0.38 0.22 7.05 1.09         4.80
Red copper oxide Colorant                                      
Red Dalton Clay 63.20 18.30   0.50 0.30         1.60 1.20   6.30 1.30         6.40
Red iron oxide, RIO Colorant                         95.00           5.00
Red Lead Flux                                   97.67 2.33
Ingredient Type Parent SiO2 Al2O3 B2O3 MgO CaO SrO BaO ZnO Li2O K2O Na2O P2O5 Fe2O3 TiO2 MnO MnO2 F PbO LOI
Red stain Colorant                                      
Redart, Red Art Clay 64.95 15.51   1.59 0.26         4.15 0.38 0.22 7.05 1.09         4.80
Rhyolite Miscellaneous 76.23 11.60   0.50 1.16         4.90 2.80   2.60 0.20          
Rice hull ash Ash 96.00 1.00   0.22 0.48         0.90 0.26 0.02 0.04 0.16 0.19       0.96
Rice straw ash Ash 82.18 1.36   1.35 3.69         2.48 0.36 0.68 0.42           7.10
Roseville Clay Clay 60.88 23.41   0.21 0.37         2.51 0.31   2.13 1.67         8.51
Rotten stone Feldspar 66.44 19.37   3.20                 9.90           1.09
Rutile Colorant                         9.90 90.00         0.10
Rye straw ash Ash 57.11 15.57   1.25 3.33         18.12   2.81 1.81            
Salt, sodium chloride Flux                     53.00               47.00
Ingredient Type Parent SiO2 Al2O3 B2O3 MgO CaO SrO BaO ZnO Li2O K2O Na2O P2O5 Fe2O3 TiO2 MnO MnO2 F PbO LOI
Sand Silica 100.00                                    
Selenium Colorant                                      
Shale Clay 61.20 19.60   1.30 0.40         3.70 1.40   7.40 1.00         4.60
Sheffield clay Clay 51.02 19.58   3.53 3.20         4.05 1.20   8.46 0.97         7.99
Sil-o-spar Feldspar 77.57 13.51     1.05         2.87 4.87   0.06           0.07
Silica, Quartz, Flint Silica 100.00                                    
Silicon carbide Silica 149.80                                    
Sillimanite Clay 37.08 62.92                                  
Silver carbonate Colorant                                      
Silver chloride Colorant                                      
Ingredient Type Parent SiO2 Al2O3 B2O3 MgO CaO SrO BaO ZnO Li2O K2O Na2O P2O5 Fe2O3 TiO2 MnO MnO2 F PbO LOI
Silver nitrate Colorant                                      
Soda Ash, Sodium Carbonate Flux                     50.00               50.00
Soda Feldspar (Theoretical) Feldspar Theoretical 68.74 19.44                 11.82                
Sodium aluminate Flux   62.19                 37.81                
Sodium antimonate Opacifier                     12.10               30.90
Sodium biborate Flux     36.50               16.30               47.20
Sodium bicarbonate Flux                     36.90                
Sodium nitrate Flux                     36.50               63.50
Sodium phosphate Flux                     19.20 22.00             58.80
Sodium selenite Colorant                     35.80                
Ingredient Type Parent SiO2 Al2O3 B2O3 MgO CaO SrO BaO ZnO Li2O K2O Na2O P2O5 Fe2O3 TiO2 MnO MnO2 F PbO LOI
Sodium silicate Flux 49.22                   50.78                
Sodium silicofluoride Flux 32.00                   33.00           60.60    
Sodium sulfate Flux                     43.60               56.40
Sodium uranate Colorant                                      
Softwood ash Flux 2.00     8.21 41.09         10.96 0.77 4.67 0.07   2.54       29.69
Sparks kaolin Clay Kaolin, China Clay (Theoretical) 46.21 37.59               0.90 0.20   0.90 0.10         14.10
Spodumene - Australian Feldspar Spodumene (Theoretical) 64.92 26.67     0.05       7.65 0.08 0.15 0.17 0.07 0.01 0.02       0.20
Spodumene - Canadian Feldspar Spodumene (Theoretical) 66.24 25.48             7.24 0.20 0.31 0.36 0.12     0.06      
Spodumene - High iron Feldspar Spodumene (Theoretical) 64.52 25.40             5.92 1.21 0.61   2.34            
Spodumene (Theoretical) Feldspar Theoretical 64.58 27.41             8.01                    
Ingredient Type Parent SiO2 Al2O3 B2O3 MgO CaO SrO BaO ZnO Li2O K2O Na2O P2O5 Fe2O3 TiO2 MnO MnO2 F PbO LOI
Spruce ash Ash 19.01 2.19   10.99 8.56         6.53 8.99 8.65 2.46           32.62
Spruce Pine #4 Feldspar 68.14 19.05     1.55         4.99 6.23   0.06            
Standard borax frit Frit 49.00 7.50 18.30   15.00         1.20 9.00                
Stannous chloride Colorant                                     20.05
Straw ash Ash 78.40     3.90 10.84             6.86              
Strontium Carbonate Flux           70.20                         29.80
Superpax Opacifier 32.78                                    
Talc, Amtalc-C98, Texas American Talc Flux Talc, Magnesium Silicate (Theoretical) 53.50 0.30   29.50 3.50         0.30     0.50 0.10         12.00
Talc, Magnesium Silicate (Theoretical) Flux Theoretical 63.38     31.87                             4.75
Tallowwood ash Ash 8.96 1.09   25.58 52.15         2.41 6.84 0.40     0.18        
Ingredient Type Parent SiO2 Al2O3 B2O3 MgO CaO SrO BaO ZnO Li2O K2O Na2O P2O5 Fe2O3 TiO2 MnO MnO2 F PbO LOI
Tennessee #1 Ball Clay Clay Ball Clay (Theoretical) 50.66 32.74   0.10 0.30         0.90 0.50   0.80 1.50         12.50
Tennessee #10 Ball Clay Clay Ball Clay (Theoretical) 52.79 30.90   0.30 0.40         0.60 0.60   1.01 1.50         11.90
Tennessee #5 Ball Clay Clay Ball Clay (Theoretical) 55.20 27.90   0.40 0.30         1.00 0.30   1.10 1.20         12.60
Tennessee #9 Ball Clay Clay Ball Clay (Theoretical) 54.20 30.10   0.40 0.50         0.40 0.30   1.10 1.60         11.40
Tennessee ball clay Clay Ball Clay (Theoretical) 54.20 30.10   0.40 0.50         0.40 0.30   1.10 1.60         11.40
Thatching grass ash Ash 76.96 5.42   3.67 6.14         2.55 0.22 1.58 1.06 0.22 0.67       1.40
Thomas Ball Clay Clay Ball Clay (Theoretical) 59.40 26.50   0.20 0.06         0.40 0.08   1.02 1.60         10.74
Tile #6 Kaolin clay Clay Kaolin, China Clay (Theoretical) 45.62 38.20   0.41 0.29           0.09   0.48 1.41         13.50
Tin Oxide, Stannic Oxide Opacifier                                      
Titanium Dioxide Opacifier                           100.00          
Ingredient Type Parent SiO2 Al2O3 B2O3 MgO CaO SrO BaO ZnO Li2O K2O Na2O P2O5 Fe2O3 TiO2 MnO MnO2 F PbO LOI
Tricalcium Phosphate, Synthetic Bone Ash Miscellaneous         54.22             45.78              
Turpentine ash Ash 89.74 1.26   1.03 1.88         1.20 4.08 0.39             0.42
Ultrox Opacifier 34.99                                    
Uranium Oxide Colorant                                      
Uranyl sodium carbonate Colorant                                      
Vanadium pentoxide Colorant                                      
Vansil W-30 Wollastonite Flux Wollastonite (Theoretical) 50.00 0.70   1.50 45.00           0.10   0.20   0.10       1.60
Veegum T Miscellaneous Montmorillonite Clay (Theoretical)                                      
Velvacast Kaolin Clay Kaolin, China Clay (Theoretical) 45.48 38.90   0.18 0.26               0.37 1.10         13.70
Vermiculite Miscellaneous 48.99 7.96   22.20 10.99       0.06                   9.80
Ingredient Type Parent SiO2 Al2O3 B2O3 MgO CaO SrO BaO ZnO Li2O K2O Na2O P2O5 Fe2O3 TiO2 MnO MnO2 F PbO LOI
Victoria Green Stain Colorant                                      
Volcanic ash - Great Plains Feldspar 72.51 11.55   0.07 0.68         7.84 1.79 0.10 1.20 0.54          
Volcanic ash - Mt. St. Helens Feldspar 63.50 18.00   2.75 5.00         1.50 4.40   5.75 0.63          
Volcanic Ash, Pumicite Feldspar 67.34 15.08   3.02 6.03         1.01 4.02 0.10 2.01 0.50         1.00
Volunteer Ball Clay Clay Ball Clay (Theoretical) 55.67 28.81   0.56 0.19         0.43 0.08   1.02 1.84         11.38
Walnut ash Ash 16.00 0.50   6.60 38.70         14.70 4.90 6.50 1.90   0.42       9.78
Wheat straw ash Ash 66.20     2.50 6.10         11.50 2.80 5.40              
Whiting, Calcium Carbonate Flux         56.10                           43.90
Willow ash Ash 4.44 0.05   8.26 20.21         49.80 2.50 10.00 1.25   0.18        
Wollastonite (Theoretical) Flux Theoretical 51.72       48.28                            
Ingredient Type Parent SiO2 Al2O3 B2O3 MgO CaO SrO BaO ZnO Li2O K2O Na2O P2O5 Fe2O3 TiO2 MnO MnO2 F PbO LOI
Wood ash Ash 19.84 1.44   6.64 20.84         22.07 6.82 13.63 8.72            
XX Sagger Ball Clay Clay Ball Clay (Theoretical) 56.73 29.17   0.30 0.50         0.89 0.30   0.69 1.71         9.71
Yankee feldspar Feldspar Potash Feldspar (Theoretical) 69.32 17.23               10.21 3.16   0.08            
Yellow Banks #101 Clay 62.28 19.48   1.12 0.90         0.02 3.26   4.61 0.93         6.07
Yellow Banks #401 Clay 54.61 30.91   0.97 0.38         0.01 0.03   1.46 0.82         10.66
Yellow iron oxide Colorant                         88.00           12.00
Yellow Ochre Colorant 57.81 19.93   0.06 0.23               21.97            
Yellow stain Colorant                                      
Zinc carbonate Flux               64.91                     35.09
Zinc Oxide Flux               100.00                      
Ingredient Type Parent SiO2 Al2O3 B2O3 MgO CaO SrO BaO ZnO Li2O K2O Na2O P2O5 Fe2O3 TiO2 MnO MnO2 F PbO LOI
Zirconium dioxide Opacifier                                      
Zircopax, Zirconium silicate Opacifier 32.78