Category: Glaze > Iron
Created 2017-07-18 09:50:42 by Tom Demeranville
Categories: Glaze > Iron
Firing Temperature: Δ6
Atmospheres: Oxidation
Surface Type: Glossy - Semi
Transparency: Opaque

This came out much more yellow than the last batch. I've a feeling I added less iron than I should have. Anyway, I really like it!

Material Amount Batch Subtotal
Silica 32.8
Nepheline Syenite (Theoretical) 16.6
Potclays/BPS High Alkaline Frit 14
Dolomite 10.8
Bone Ash 10.3
Whiting 8.5
Lithium Carbonate 5.7
Gillespie Borate 1.3
Total Base:100
Iron oxide 20
Bentonite 2
Total: 122

Percentage Analysis

Ingredient Amount SiO2 Al2O3 B2O3 MgO CaO SrO Li2O K2O Na2O KNaO P2O5 Fe2O3 LOI
Silica32.832.8
Nepheline Syenite (Theoretical)16.610.083.870.020.120.761.632.390.020.12
Potclays/BPS High Alkaline Frit147.040.80.540.742.432.444.87
Dolomite10.82.373.295.14
Bone Ash10.35.754.370.18
Whiting8.54.773.73
Lithium Carbonate5.72.323.38
Gillespie Borate1.30.150.020.320.050.30.010.050.050.4
Iron oxide20191
Bentonite21.190.40.040.020.020.060.080.070.2
Total12251.265.090.862.4714.990.012.323.214.187.394.3719.0914.15
100% no LOI 47.534.720.82.2913.90.012.152.983.886.864.0517.7

Unity Molecular Formula (UMF)

FLUXES

RO/R2O

0.13 Na2O
0.07 K2O
0.15 Li2O
0.53 CaO
0.12 MgO
STABILIZERS

R2O3

0.1 Al2O3
0.02 B2O3
GLASS-FORMERS

RO2

1.68 SiO2
OTHER

 

0.24 Fe2O3
0.06 P2O5
SILICA:ALUMINA

SiO2:Al2O3

17.09

FLUX RATIO

R2O:RO

0.35 : 0.65

SiO2:Al2O3 Chart

Closest 100 neighbors in Glaze > Iron.

Click and drag to zoom
Stull Chart
SiO2:Al2O3 Ratio
SiO2:Al2O3 Ratio 17.09

Similar Base Recipes

No recipes with similar base ingredients and amounts were found.

Similar RO/R2O Unity Formulas

R2O3 - STABILIZERS RO2 - GLASS FORMERS RO/R2O - FLUXES
Recipe Name ΔTemp Al2O3 B2O3 SiO2 ZrO2 SnO2 TiO2 KNaO K2O Na2O CaO MgO ZnO BaO PbO Li2O SrO
John's Straw Ash (Toms GB variation) 6 0.1 0.02 1.68 0.2 0.07 0.13 0.53 0.12 0.15
John's Straw Ash 6 0.1 0.02 1.64 0.21 0.03 0.18 0.53 0.11 0.15
John's Straw Ash 5-6 0.1 0.02 1.65 0.21 0.03 0.18 0.53 0.11 0.15

No reviews yet.

Hazards

09/2016 Note: This is a new feature. If a recipe material is not listed, that material's data has not yet been added. Some materials only have GHS ratings, while others only have HMIS ratings. Warnings differ between systems and countries. Glazy does not take any responsibility for accuracy of linked SDS information. Contact your ceramics supplier for safety information for your specific materials.
Globally Harmonized System (GHS) Hazardous Materials Identification System (HMIS) SDS Link
Material Pictograms Signal Word Hazard Statements Health Flammability Hazard Protection
Silica HarmfulHealth Hazard DANGER From 200-Mesh SDS:
May cause cancer by inhalation.
Causes damage to lungs through prolonged or repeated exposure by inhalation.
* 0 0 E
Dolomite Health Hazard DANGER May cause cancer (Inhalation) 1 0 0 E
Bone Ash
Whiting Harmful WARNING Causes eye irritation
Lithium Carbonate Harmful WARNING Harmful if swallowed.
Causes serious eye irritation.
Harmful to aquatic life.
Iron oxide Health Hazard WARNING SDS for Red Iron Oxide: May cause damage to lung through prolonged or repeated exposure by inhalation
Bentonite Harmful WARNING Causes eye irritation
Causes skin irritation
May cause respiratory irritation