Category: Glaze > Turquoise
Created 2017-07-30 19:34:23 by Clara Giorello
Categories: Glaze > Turquoise
Firing Temperature: Δ6
Atmospheres: Oxidation
Surface Type: Matte - Smooth
Transparency: Semi-opaque

Material Amount Batch Subtotal
Potash Feldspar (Theoretical) 45.36
Dolomite 18.14
Kaolin (Theoretical) 18.14
Crecer Frit 804 9.29
Soda Ash 9.07
Total Base:100
Tin Oxide 1.92
Bentonite 1.92
Copper Carbonate 1.44
Total: 105.28

Percentage Analysis

Ingredient Amount SiO2 Al2O3 B2O3 MgO CaO K2O Na2O KNaO Fe2O3 TiO2 CuO SnO2 LOI
Potash Feldspar (Theoretical)45.3629.388.317.677.67
Dolomite18.143.975.538.64
Kaolin (Theoretical)18.148.587.292.27
Crecer Frit 8049.295.030.861.020.060.60.331.211.540.030.010.14
Soda Ash9.074.544.544.54
Tin Oxide1.921.92
Bentonite1.921.140.390.040.020.020.060.080.070.19
Copper Carbonate1.440.930.51
Total105.2844.1216.851.024.076.158.035.8113.830.090.010.931.9216.28
100% no LOI 49.5718.941.154.576.919.026.5215.540.110.011.042.16

Unity Molecular Formula (UMF)

FLUXES

RO/R2O

0.24 Na2O
0.22 K2O
0.28 CaO
0.26 MgO
STABILIZERS

R2O3

0.42 Al2O3
0.04 B2O3
GLASS-FORMERS

RO2

1.88 SiO2
0.03 SnO2
OTHER

 

0.03 CuO
SILICA:ALUMINA

SiO2:Al2O3

4.44

FLUX RATIO

R2O:RO

0.46 : 0.54

SiO2:Al2O3 Chart

Closest 67 neighbors in Glaze > Turquoise.

Click and drag to zoom
Stull Chart
SiO2:Al2O3 Ratio
SiO2:Al2O3 Ratio 4.44

Similar Base Recipes

No recipes with similar base ingredients and amounts were found.

Similar RO/R2O Unity Formulas

R2O3 - STABILIZERS RO2 - GLASS FORMERS RO/R2O - FLUXES
Recipe Name ΔTemp Al2O3 B2O3 SiO2 ZrO2 SnO2 TiO2 KNaO K2O Na2O CaO MgO ZnO BaO PbO Li2O SrO
Turquoise Matte 2 6 0.42 0.04 1.88 0.03 0.46 0.22 0.24 0.28 0.26
Turquoise Matte 1 6 0.43 0.02 1.87 0.03 0.45 0.22 0.23 0.28 0.27

No reviews yet.

Hazards

09/2016 Note: This is a new feature. If a recipe material is not listed, that material's data has not yet been added. Some materials only have GHS ratings, while others only have HMIS ratings. Warnings differ between systems and countries. Glazy does not take any responsibility for accuracy of linked SDS information. Contact your ceramics supplier for safety information for your specific materials.
Globally Harmonized System (GHS) Hazardous Materials Identification System (HMIS) SDS Link
Material Pictograms Signal Word Hazard Statements Health Flammability Hazard Protection
Dolomite Health Hazard DANGER May cause cancer (Inhalation) 1 0 0 E
Kaolin (Theoretical) HarmfulHealth Hazard DANGER SDS for EPK KAOLIN: EPK Kaolin is a naturally occurring mineral, which may contain amounts of crystalline silica
typically 0.1-1.0%, may cause damage to respiratory system through prolonged or repeated
exposure.
Soda Ash Harmful WARNING Causes skin irritation.
Causes serious eye irritation.
2 0 0 B
Tin Oxide Harmful WARNING Harmful if swallowed.
Bentonite Harmful WARNING Causes eye irritation
Causes skin irritation
May cause respiratory irritation
Copper Carbonate Harmful WARNING Harmful if swallowed.
Causes skin irritation.
Causes serious eye irritation.