Material Amount Batch Subtotal
Silica 35.4
Frit 3134 29.2
Nepheline Syenite (Theoretical) 20
EPK 6.6
Strontium Carbonate 5.7
Wollastonite (Theoretical) 2.5
Dolomite 0.6
Total Base:100
Tin Oxide 2
Bentonite 2
Copper Carbonate 1.5
Silicon carbide 0.8
Total: 106.3

Percentage Analysis

Ingredient Amount SiO2 Al2O3 B2O3 MgO CaO SrO K2O Na2O KNaO P2O5 Fe2O3 TiO2 CuO SnO2 LOI
Silica35.435.4
Frit 313429.213.586.745.8833
Nepheline Syenite (Theoretical)2012.144.660.020.140.921.962.880.020.14
EPK6.63.022.470.010.010.020.020.020.050.030.98
Strontium Carbonate5.741.7
Wollastonite (Theoretical)2.51.291.21
Dolomite0.60.130.180.29
Tin Oxide22
Bentonite21.190.40.040.020.020.060.080.070.2
Copper Carbonate1.50.970.53
Silicon carbide0.81.2
Total106.367.827.536.740.27.4440.965.035.990.020.140.030.9723.44
100% no LOI 65.937.326.550.197.233.890.944.895.820.020.140.020.941.94

Unity Molecular Formula (UMF)

FLUXES

RO/R2O

0.3 Na2O
0.04 K2O
0.14 SrO
0.5 CaO
0.02 MgO
STABILIZERS

R2O3

0.28 Al2O3
0.36 B2O3
GLASS-FORMERS

RO2

4.14 SiO2
0.05 SnO2
OTHER

 

0.05 CuO
SILICA:ALUMINA

SiO2:Al2O3

15.02

FLUX RATIO

R2O:RO

0.34 : 0.66

SiO2:Al2O3 Chart

Closest 100 neighbors in Glaze > Red > Copper.

Click and drag to zoom
Stull Chart
SiO2:Al2O3 Ratio
SiO2:Al2O3 Ratio 15.02

Similar Base Recipes

Similar RO/R2O Unity Formulas

R2O3 - STABILIZERS RO2 - GLASS FORMERS RO/R2O - FLUXES
Recipe Name ΔTemp Al2O3 B2O3 SiO2 ZrO2 SnO2 TiO2 KNaO K2O Na2O CaO MgO ZnO BaO PbO Li2O SrO
A2V / frit Copper SiC Red 6 0.28 0.36 4.14 0.05 0.34 0.04 0.3 0.5 0.02 0.14
Heath A2V Base /frit 5-5½ 0.26 0.37 4.11 0.34 0.04 0.3 0.5 0.01 0.15
Heath A2V /frit SiC Chun 5½-6 0.28 0.36 4.14 0.34 0.04 0.3 0.5 0.02 0.14

No reviews yet.

Hazards

09/2016 Note: This is a new feature. If a recipe material is not listed, that material's data has not yet been added. Some materials only have GHS ratings, while others only have HMIS ratings. Warnings differ between systems and countries. Glazy does not take any responsibility for accuracy of linked SDS information. Contact your ceramics supplier for safety information for your specific materials.
Globally Harmonized System (GHS) Hazardous Materials Identification System (HMIS) SDS Link
Material Pictograms Signal Word Hazard Statements Health Flammability Hazard Protection
Silica HarmfulHealth Hazard DANGER From 200-Mesh SDS:
May cause cancer by inhalation.
Causes damage to lungs through prolonged or repeated exposure by inhalation.
* 0 0 E
EPK HarmfulHealth Hazard DANGER EPK Kaolin is a naturally occurring mineral, which may contain amounts of crystalline silica
typically 0.1-1.0%, may cause damage to respiratory system through prolonged or repeated
exposure.
1 0 0 E
Strontium Carbonate Harmful WARNING Product dust may be irritating to eyes,skin and respiratory system.  1 0 0 E
Wollastonite (Theoretical) Health Hazard DANGER Vansil W-30 Wollastonite SDS:
May cause cancer if inhaled.
Causes damage to organs through prolonged or repeated exposure if inhaled. (respiratory tract)
Dolomite Health Hazard DANGER May cause cancer (Inhalation) 1 0 0 E
Tin Oxide Harmful WARNING Harmful if swallowed.
Bentonite Harmful WARNING Causes eye irritation
Causes skin irritation
May cause respiratory irritation
Copper Carbonate Harmful WARNING Harmful if swallowed.
Causes skin irritation.
Causes serious eye irritation.
Silicon carbide Health Hazard WARNING May cause cancer