Category: Glaze > Iron > Oil Spot
Created 2017-08-03 08:06:03 by Pieter Mostert
Categories: Glaze > Iron > Oil Spot
Firing Temperature: Δ4
Atmospheres: Oxidation
Surface Type: Glossy
Transparency: Opaque

Average of "Overberg Oilspot (more alumina, more silica) (more MgO less CaO variation)" and "Overberg Oilspot (more alumina, more silica) (less MgO more CaO variation)"

Material Amount Batch Subtotal
Refined Overberg Earthenware 40.5
Frit FSB 510 Na2O 21.5
Talc - Magsil 13.8
Kaolin G (Serina ML Pellets) 7.6
Silica 7
Wollastonite (Theoretical) 6.1
Nepheline Syenite, North Cape 3.6
Total Base:100.1
Red iron oxide 7.7
Total: 107.8

Percentage Analysis

Ingredient Amount SiO2 Al2O3 B2O3 MgO CaO SrO BaO K2O Na2O KNaO Fe2O3 TiO2 LOI
Refined Overberg Earthenware40.523.857.90.280.890.893.690.533.69
Frit FSB 510 Na2O21.59.610.456.192.492.752.75
Talc - Magsil13.88.460.024.310.130.020.020.080.73
Kaolin G (Serina ML Pellets)7.63.542.610.020.010.140.010.150.021.25
Silica77
Wollastonite (Theoretical)6.13.162.94
Nepheline Syenite, North Cape3.62.010.880.040.010.010.320.280.60.03
Red iron oxide7.77.320.39
Total107.857.6411.866.194.65.610.010.011.363.064.4211.110.536.08
100% no LOI 56.5211.636.074.515.50.010.011.3434.3410.890.52

Unity Molecular Formula (UMF)

FLUXES

RO/R2O

0.18 Na2O
0.05 K2O
0.36 CaO
0.41 MgO
STABILIZERS

R2O3

0.42 Al2O3
0.32 B2O3
GLASS-FORMERS

RO2

3.44 SiO2
0.02 TiO2
OTHER

 

0.25 Fe2O3
SILICA:ALUMINA

SiO2:Al2O3

8.27

FLUX RATIO

R2O:RO

0.23 : 0.77

SiO2:Al2O3 Chart

Closest 26 neighbors in Glaze > Iron > Oil Spot.

Click and drag to zoom
Stull Chart
SiO2:Al2O3 Ratio
SiO2:Al2O3 Ratio 8.27

Similar Base Recipes

No recipes with similar base ingredients and amounts were found.

Similar RO/R2O Unity Formulas

No recipes with similar RO/R2O Unity Formulas were found.

No reviews yet.

Hazards

09/2016 Note: This is a new feature. If a recipe material is not listed, that material's data has not yet been added. Some materials only have GHS ratings, while others only have HMIS ratings. Warnings differ between systems and countries. Glazy does not take any responsibility for accuracy of linked SDS information. Contact your ceramics supplier for safety information for your specific materials.
Globally Harmonized System (GHS) Hazardous Materials Identification System (HMIS) SDS Link
Material Pictograms Signal Word Hazard Statements Health Flammability Hazard Protection
Silica HarmfulHealth Hazard DANGER From 200-Mesh SDS:
May cause cancer by inhalation.
Causes damage to lungs through prolonged or repeated exposure by inhalation.
* 0 0 E
Wollastonite (Theoretical) Health Hazard DANGER Vansil W-30 Wollastonite SDS:
May cause cancer if inhaled.
Causes damage to organs through prolonged or repeated exposure if inhaled. (respiratory tract)
Red iron oxide Health Hazard WARNING May cause damage to lung through prolonged or repeated exposure by inhalation