Category: Glaze > Crystalline > Micro
Created 2017-08-05 22:05:07 by Rod Haaland
Categories: Glaze > Crystalline > Micro
Firing Temperature: Δ5½-6
Atmospheres: Oxidation
Surface Type: Glossy - Semi
Transparency: Translucent

Cone Six Oxidation - Satin / Matt / Gloss
Microcrystalline.

Material Amount Batch Subtotal
Frit 3110 39.3
Spodumene - Australian 31.5
Whiting 9.8
Red iron oxide 7.9
Frit 3134 7.1
Titanium Dioxide 4.4
Bentonite 2
Total: 102

Percentage Analysis

Ingredient Amount SiO2 Al2O3 B2O3 MgO CaO Li2O K2O Na2O KNaO P2O5 Fe2O3 TiO2 MnO LOI
Frit 311039.326.282.371.142.221.355.947.29
Spodumene - Australian31.520.458.40.022.410.030.050.080.050.020.010.06
Whiting9.85.54.3
Red iron oxide7.97.510.4
Frit 31347.13.31.641.430.730.73
Titanium Dioxide4.44.4
Bentonite21.190.40.040.020.020.060.080.070.2
Total10251.2211.172.780.049.182.411.46.788.180.057.64.40.014.96
100% no LOI 52.7911.512.860.049.462.481.446.988.430.067.834.540.01

Unity Molecular Formula (UMF)

FLUXES

RO/R2O

0.3 Na2O
0.04 K2O
0.22 Li2O
0.44 CaO
STABILIZERS

R2O3

0.3 Al2O3
0.11 B2O3
GLASS-FORMERS

RO2

2.31 SiO2
0.15 TiO2
OTHER

 

0.13 Fe2O3
SILICA:ALUMINA

SiO2:Al2O3

7.78

FLUX RATIO

R2O:RO

0.55 : 0.45

SiO2:Al2O3 Chart

Closest 7 neighbors in Glaze > Crystalline > Micro.

Click and drag to zoom
Stull Chart
SiO2:Al2O3 Ratio
SiO2:Al2O3 Ratio 7.78

Similar Base Recipes

No recipes with similar base ingredients and amounts were found.

Similar RO/R2O Unity Formulas

No recipes with similar RO/R2O Unity Formulas were found.

No reviews yet.

Hazards

09/2016 Note: This is a new feature. If a recipe material is not listed, that material's data has not yet been added. Some materials only have GHS ratings, while others only have HMIS ratings. Warnings differ between systems and countries. Glazy does not take any responsibility for accuracy of linked SDS information. Contact your ceramics supplier for safety information for your specific materials.
Globally Harmonized System (GHS) Hazardous Materials Identification System (HMIS) SDS Link
Material Pictograms Signal Word Hazard Statements Health Flammability Hazard Protection
Whiting Harmful WARNING Causes eye irritation
Red iron oxide Health Hazard WARNING May cause damage to lung through prolonged or repeated exposure by inhalation
Titanium Dioxide Health Hazard WARNING Suspected of causing cancer
Bentonite Harmful WARNING Causes eye irritation
Causes skin irritation
May cause respiratory irritation