Category: Glaze > White, Off-White
Created 2017-08-07 02:21:49 by Clara Giorello
Categories: Glaze > White, Off-White
Firing Temperature: Δ5½
Atmospheres: Oxidation
Surface Type: Matte
Transparency: Semi-opaque

Material Amount Batch Subtotal
Potash Feldspar (Theoretical) 88.93
Whiting 5.9
Strontium Carbonate 4.94
Silica 0.23
Total: 100

Percentage Analysis

Ingredient Amount SiO2 Al2O3 CaO SrO K2O KNaO LOI
Potash Feldspar (Theoretical)88.9357.5916.2915.0515.05
Whiting5.93.312.59
Strontium Carbonate4.943.471.47
Silica0.230.23
Total10057.8216.293.313.4715.0515.054.06
100% no LOI 60.2716.983.453.6115.6815.68

Unity Molecular Formula (UMF)

FLUXES

RO/R2O

0.63 K2O
0.13 SrO
0.23 CaO
STABILIZERS

R2O3

0.63 Al2O3
GLASS-FORMERS

RO2

3.82 SiO2
SILICA:ALUMINA

SiO2:Al2O3

6.02

FLUX RATIO

R2O:RO

0.63 : 0.37

SiO2:Al2O3 Chart

Closest 100 neighbors in Glaze > White, Off-White.

Click and drag to zoom
Stull Chart
SiO2:Al2O3 Ratio
SiO2:Al2O3 Ratio 6.02

Similar Base Recipes

No recipes with similar base ingredients and amounts were found.

Similar RO/R2O Unity Formulas

No recipes with similar RO/R2O Unity Formulas were found.

No reviews yet.

Hazards

09/2016 Note: This is a new feature. If a recipe material is not listed, that material's data has not yet been added. Some materials only have GHS ratings, while others only have HMIS ratings. Warnings differ between systems and countries. Glazy does not take any responsibility for accuracy of linked SDS information. Contact your ceramics supplier for safety information for your specific materials.
Globally Harmonized System (GHS) Hazardous Materials Identification System (HMIS) SDS Link
Material Pictograms Signal Word Hazard Statements Health Flammability Hazard Protection
Whiting Harmful WARNING Causes eye irritation
Strontium Carbonate Harmful WARNING Product dust may be irritating to eyes,skin and respiratory system.  1 0 0 E
Silica HarmfulHealth Hazard DANGER From 200-Mesh SDS:
May cause cancer by inhalation.
Causes damage to lungs through prolonged or repeated exposure by inhalation.
* 0 0 E