Material Amount Batch Subtotal
Mahavir Potash Feldspar 47.56
EPK 25.3
Whiting 17.02
Frit 3134 10.12
Total Base:100
Copper Carbonate 4
Titanium Dioxide 4
Total: 108

Percentage Analysis

Ingredient Amount SiO2 Al2O3 B2O3 MgO CaO K2O Na2O KNaO P2O5 Fe2O3 TiO2 CuO LOI
Mahavir Potash Feldspar47.5631.878.320.070.075.471.436.90.040.24
EPK25.311.579.450.030.050.090.020.110.070.190.13.75
Whiting17.029.557.47
Frit 313410.124.712.342.041.041.04
Copper Carbonate42.581.42
Titanium Dioxide44
Total10848.1417.782.340.111.75.562.488.040.070.234.12.5812.88
100% no LOI 50.6418.72.460.112.315.852.618.460.070.244.312.71

Unity Molecular Formula (UMF)

FLUXES

RO/R2O

0.13 Na2O
0.19 K2O
0.67 CaO
0.01 MgO
STABILIZERS

R2O3

0.56 Al2O3
0.11 B2O3
GLASS-FORMERS

RO2

2.58 SiO2
0.17 TiO2
OTHER

 

0.1 CuO
SILICA:ALUMINA

SiO2:Al2O3

4.60

FLUX RATIO

R2O:RO

0.32 : 0.68

SiO2:Al2O3 Chart

Closest 100 neighbors in Glaze > Green > Copper.

Click and drag to zoom
Stull Chart
SiO2:Al2O3 Ratio
SiO2:Al2O3 Ratio 4.6

Similar Base Recipes

No recipes with similar base ingredients and amounts were found.

Similar RO/R2O Unity Formulas

No recipes with similar RO/R2O Unity Formulas were found.

No reviews yet.

Hazards

09/2016 Note: This is a new feature. If a recipe material is not listed, that material's data has not yet been added. Some materials only have GHS ratings, while others only have HMIS ratings. Warnings differ between systems and countries. Glazy does not take any responsibility for accuracy of linked SDS information. Contact your ceramics supplier for safety information for your specific materials.
Globally Harmonized System (GHS) Hazardous Materials Identification System (HMIS) SDS Link
Material Pictograms Signal Word Hazard Statements Health Flammability Hazard Protection
EPK HarmfulHealth Hazard DANGER EPK Kaolin is a naturally occurring mineral, which may contain amounts of crystalline silica
typically 0.1-1.0%, may cause damage to respiratory system through prolonged or repeated
exposure.
1 0 0 E
Whiting Harmful WARNING Causes eye irritation
Copper Carbonate Harmful WARNING Harmful if swallowed.
Causes skin irritation.
Causes serious eye irritation.
Titanium Dioxide Health Hazard WARNING Suspected of causing cancer