Category: Glaze > Shino > Carbon Trap
Created 2017-08-26 21:56:09 by Ken Potter
Categories: Glaze > Shino > Carbon Trap
Firing Temperature: Δ10
Atmospheres: Reduction
Surface Type: Glossy
Transparency: Semi-opaque

I know there must hundreds if not thousands of Carbon Trap Shinos out there. So here here is my contribution to the chaos.
I have added 3% Red Iron Oxide to give color and a bit of luster.

Material Amount Batch Subtotal
Kona F-4 feldspar 68
Spodumene (Theoretical) 15
EPK 12
Soda Ash 5
Total Base:100
Red iron oxide 3
Bentonite 1
Total: 104

Percentage Analysis

Ingredient Amount SiO2 Al2O3 MgO CaO Li2O K2O Na2O KNaO P2O5 Fe2O3 TiO2 LOI
Kona F-4 feldspar6845.3813.320.031.163.264.697.950.030.14
Spodumene (Theoretical)159.694.111.2
EPK125.494.480.010.020.040.010.050.030.090.051.78
Soda Ash52.52.52.5
Red iron oxide32.850.15
Bentonite10.590.20.020.010.010.030.040.040.1
Total10461.1522.110.071.191.23.317.2310.540.0330.054.66
100% no LOI 61.5622.260.071.21.213.337.2710.610.033.020.05

Unity Molecular Formula (UMF)

FLUXES

RO/R2O

0.54 Na2O
0.16 K2O
0.19 Li2O
0.1 CaO
0.01 MgO
STABILIZERS

R2O3

1.01 Al2O3
GLASS-FORMERS

RO2

4.74 SiO2
OTHER

 

0.09 Fe2O3
SILICA:ALUMINA

SiO2:Al2O3

4.69

FLUX RATIO

R2O:RO

0.89 : 0.11

SiO2:Al2O3 Chart

Closest 19 neighbors in Glaze > Shino > Carbon Trap.

Click and drag to zoom
Stull Chart
SiO2:Al2O3 Ratio
SiO2:Al2O3 Ratio 4.69

Similar Base Recipes

No recipes with similar base ingredients and amounts were found.

Similar RO/R2O Unity Formulas

R2O3 - STABILIZERS RO2 - GLASS FORMERS RO/R2O - FLUXES
Recipe Name ΔTemp Al2O3 B2O3 SiO2 ZrO2 SnO2 TiO2 KNaO K2O Na2O CaO MgO ZnO BaO PbO Li2O SrO
Shino 7 Gold 10 1.01 4.74 0.7 0.16 0.54 0.1 0.01 0.19
Shino Kansas City no spod 10 1.04 4.74 0.73 0.17 0.56 0.08 0.01 0.18

No reviews yet.

Hazards

09/2016 Note: This is a new feature. If a recipe material is not listed, that material's data has not yet been added. Some materials only have GHS ratings, while others only have HMIS ratings. Warnings differ between systems and countries. Glazy does not take any responsibility for accuracy of linked SDS information. Contact your ceramics supplier for safety information for your specific materials.
Globally Harmonized System (GHS) Hazardous Materials Identification System (HMIS) SDS Link
Material Pictograms Signal Word Hazard Statements Health Flammability Hazard Protection
Spodumene (Theoretical) Health Hazard DANGER May cause cancer by inhalation.
Causes damage to organs through prolonged or repeated exposure.
EPK HarmfulHealth Hazard DANGER EPK Kaolin is a naturally occurring mineral, which may contain amounts of crystalline silica
typically 0.1-1.0%, may cause damage to respiratory system through prolonged or repeated
exposure.
1 0 0 E
Soda Ash Harmful WARNING Causes skin irritation.
Causes serious eye irritation.
2 0 0 B
Red iron oxide Health Hazard WARNING May cause damage to lung through prolonged or repeated exposure by inhalation
Bentonite Harmful WARNING Causes eye irritation
Causes skin irritation
May cause respiratory irritation