Category: Glaze > Crystalline > Manganese
Created 2017-08-30 21:38:06 by Ken Potter
Categories: Glaze > Crystalline > Manganese
Firing Temperature: Δ10
Atmospheres: Oxidation, Neutral, Reduction
Surface Type: Glossy - Semi
Transparency: Opaque

From John Brett's book The Complete Guide To High-Fire Glazes.
10% Redart added to reduce the running.

Material Amount Batch Subtotal
Custer Feldspar 100
Total Base:100
Manganese Dioxide 26.5
Redart 10
Bentonite 3
Total: 139.5

Percentage Analysis

Ingredient Amount SiO2 Al2O3 MgO CaO K2O Na2O KNaO P2O5 Fe2O3 TiO2 MnO2 LOI
Custer Feldspar10068.5170.3103130.10.3
Manganese Dioxide26.523.033.47
Redart106.51.550.160.030.410.040.450.020.70.110.48
Bentonite31.780.60.060.030.030.090.120.110.3
Total139.576.7719.150.220.3610.453.1313.570.020.910.1123.034.55
100% no LOI 57.2314.280.160.277.792.3310.120.020.680.0817.17

Unity Molecular Formula (UMF)

FLUXES

RO/R2O

0.29 Na2O
0.64 K2O
0.04 CaO
0.03 MgO
STABILIZERS

R2O3

1.08 Al2O3
GLASS-FORMERS

RO2

7.38 SiO2
0.01 TiO2
OTHER

 

0.03 Fe2O3
1.52 MnO2
SILICA:ALUMINA

SiO2:Al2O3

6.80

FLUX RATIO

R2O:RO

0.93 : 0.07

SiO2:Al2O3 Chart

Closest 6 neighbors in Glaze > Crystalline > Manganese.

Click and drag to zoom
Stull Chart
SiO2:Al2O3 Ratio
SiO2:Al2O3 Ratio 6.8

Similar Base Recipes

Similar RO/R2O Unity Formulas

No recipes with similar RO/R2O Unity Formulas were found.

No reviews yet.

Hazards

09/2016 Note: This is a new feature. If a recipe material is not listed, that material's data has not yet been added. Some materials only have GHS ratings, while others only have HMIS ratings. Warnings differ between systems and countries. Glazy does not take any responsibility for accuracy of linked SDS information. Contact your ceramics supplier for safety information for your specific materials.
Globally Harmonized System (GHS) Hazardous Materials Identification System (HMIS) SDS Link
Material Pictograms Signal Word Hazard Statements Health Flammability Hazard Protection
Custer Feldspar HarmfulHealth Hazard WARNING May cause damage to lungs through prolonged or repeated inhalation.
Suspected of causing cancer through
prolonged or repeated inhalation.
May cause allergy or asthma symptoms or breathing difficulties if inhaled.
May cause skin or eye irritation.
Manganese Dioxide Harmful WARNING Harmful if swallowed. Causes serious eye irritation. Harmful if inhaled. May cause respiratory
irritation.
Redart HarmfulHealth Hazard DANGER Causes skin irritation
Causes eye irritation
May cause cancer (Inhalation)
Bentonite Harmful WARNING Causes eye irritation
Causes skin irritation
May cause respiratory irritation