Cedar Hill Studio old Lavender recipe... this is what the old Lavender should have been, with the missing ingredients included. Not quite the colour we wanted and I don't like the chemistry so I made a new Lavender recipe.

Material Amount Batch Subtotal
Silica 30
Gerstley Borate 21
Nepheline Syenite (Theoretical) 12
Amtalc-C98 Talc 12
Dolomite 12
Kentucky OM #4 Ball Clay 8
Spodumene - Canadian 5
Total Base:100
Cobalt Carbonate 2
Total: 102

Percentage Analysis

Ingredient Amount SiO2 Al2O3 B2O3 MgO CaO Li2O K2O Na2O KNaO P2O5 Fe2O3 TiO2 MnO2 CoO LOI
Silica3030
Gerstley Borate213.110.215.630.734.070.080.840.920.020.080.026.2
Nepheline Syenite (Theoretical)127.282.80.010.080.551.181.730.010.08
Amtalc-C98 Talc126.420.043.540.420.040.040.060.011.44
Dolomite122.633.665.71
Kentucky OM #4 Ball Clay84.422.230.030.020.080.020.10.090.11.01
Spodumene - Canadian53.311.270.360.010.020.030.020.01
Cobalt Carbonate21.260.74
Total10254.546.555.636.958.260.360.762.062.820.040.250.1301.2615.18
100% no LOI 62.857.556.488.019.520.420.882.373.250.040.290.1501.45

Unity Molecular Formula (UMF)

FLUXES

RO/R2O

0.09 Na2O
0.02 K2O
0.03 Li2O
0.39 CaO
0.46 MgO
STABILIZERS

R2O3

0.17 Al2O3
0.22 B2O3
GLASS-FORMERS

RO2

2.43 SiO2
OTHER

 

0.05 CoO
SILICA:ALUMINA

SiO2:Al2O3

14.14

FLUX RATIO

R2O:RO

0.14 : 0.86

SiO2:Al2O3 Chart

Closest 100 neighbors in Glaze.

Click and drag to zoom
Stull Chart
SiO2:Al2O3 Ratio
SiO2:Al2O3 Ratio 14.14

Similar Base Recipes

Similar RO/R2O Unity Formulas

R2O3 - STABILIZERS RO2 - GLASS FORMERS RO/R2O - FLUXES
Recipe Name ΔTemp Al2O3 B2O3 SiO2 ZrO2 SnO2 TiO2 KNaO K2O Na2O CaO MgO ZnO BaO PbO Li2O SrO
Lavender - old - full recipe (Cedar Hill) 6 0.17 0.22 2.43 0.11 0.02 0.09 0.39 0.46 0.03
Bob's S-2 Glaze 7-8 0.19 0.25 2.43 0.11 0.02 0.09 0.41 0.48

No reviews yet.

Hazards

09/2016 Note: This is a new feature. If a recipe material is not listed, that material's data has not yet been added. Some materials only have GHS ratings, while others only have HMIS ratings. Warnings differ between systems and countries. Glazy does not take any responsibility for accuracy of linked SDS information. Contact your ceramics supplier for safety information for your specific materials.
Globally Harmonized System (GHS) Hazardous Materials Identification System (HMIS) SDS Link
Material Pictograms Signal Word Hazard Statements Health Flammability Hazard Protection
Silica HarmfulHealth Hazard DANGER From 200-Mesh SDS:
May cause cancer by inhalation.
Causes damage to lungs through prolonged or repeated exposure by inhalation.
* 0 0 E
Gerstley Borate
Amtalc-C98 Talc Harmful WARNING Causes mild skin irritation
Harmful if inhaled
May cause respiratory irritation
1 0 0 E
Dolomite Health Hazard DANGER May cause cancer (Inhalation) 1 0 0 E
Kentucky OM #4 Ball Clay Health Hazard WARNING May cause damage to lung through prolonged or repeated inhalation 2 0 0 E
Cobalt Carbonate Health HazardEnvironmental Hazard DANGER May cause cancer
Suspected of causing genetic effects
May damage fertility or the unborn child
May cause allergy or breathing difficulties if inhaled
May cause a allergic skin reaction
Very toxic to aquatic life
Very toxic to aquatic life with long lasting effects
2 0 0 *