Category: Glaze
Created 2017-09-04 04:14:08 by Sue McLeod
Categories: Glaze
Firing Temperature: Δ6
Atmospheres: Oxidation
Surface Type: Matte
Transparency: Opaque

Old eggplant glaze removed from CH studio due to manganese.

Material Amount Batch Subtotal
Minspar 200 45.25
Silica 15.05
Gerstley Borate 12.77
Amtalc-C98 Talc 12.57
Dolomite 8.91
EPK 4.46
Total Base:99.01
Manganese Carbonate 5
Cobalt Carbonate 2
Bentonite 1
Total: 107.01

Percentage Analysis

Ingredient Amount SiO2 Al2O3 B2O3 MgO CaO K2O Na2O KNaO P2O5 Fe2O3 TiO2 MnO CoO LOI
Minspar 20045.2531.188.410.681.862.954.810.030.14
Silica15.0515.05
Gerstley Borate12.771.890.133.420.452.480.050.510.560.010.050.013.77
Amtalc-C98 Talc12.576.720.043.710.440.040.040.060.011.51
Dolomite8.911.952.724.24
EPK4.462.041.670.010.020.020.010.030.020.66
Manganese Carbonate53.081.92
Cobalt Carbonate21.260.74
Bentonite10.590.20.020.010.010.030.040.040.1
Total107.0157.4810.443.426.136.331.983.55.480.020.210.043.081.2613.07
100% no LOI 61.2111.123.646.536.742.113.735.830.030.220.053.281.34

Unity Molecular Formula (UMF)

FLUXES

RO/R2O

0.16 Na2O
0.06 K2O
0.33 CaO
0.44 MgO
STABILIZERS

R2O3

0.3 Al2O3
0.14 B2O3
GLASS-FORMERS

RO2

2.79 SiO2
OTHER

 

0.13 MnO
0.05 CoO
SILICA:ALUMINA

SiO2:Al2O3

9.34

FLUX RATIO

R2O:RO

0.23 : 0.77

SiO2:Al2O3 Chart

Closest 100 neighbors in Glaze.

Click and drag to zoom
Stull Chart
SiO2:Al2O3 Ratio
SiO2:Al2O3 Ratio 9.34

Similar Base Recipes

No recipes with similar base ingredients and amounts were found.

Similar RO/R2O Unity Formulas

R2O3 - STABILIZERS RO2 - GLASS FORMERS RO/R2O - FLUXES
Recipe Name ΔTemp Al2O3 B2O3 SiO2 ZrO2 SnO2 TiO2 KNaO K2O Na2O CaO MgO ZnO BaO PbO Li2O SrO
Eggplant (Cedar Hill) 6 0.3 0.14 2.79 0.22 0.06 0.16 0.33 0.44
Chappell Clear Semigloss 6 0.3 0.14 2.75 0.24 0.07 0.17 0.3 0.46

No reviews yet.

Hazards

09/2016 Note: This is a new feature. If a recipe material is not listed, that material's data has not yet been added. Some materials only have GHS ratings, while others only have HMIS ratings. Warnings differ between systems and countries. Glazy does not take any responsibility for accuracy of linked SDS information. Contact your ceramics supplier for safety information for your specific materials.
Globally Harmonized System (GHS) Hazardous Materials Identification System (HMIS) SDS Link
Material Pictograms Signal Word Hazard Statements Health Flammability Hazard Protection
Minspar 200 Health Hazard WARNING May cause damage to lung through prolonged or repeated inhalation 2 0 0 E
Silica HarmfulHealth Hazard DANGER From 200-Mesh SDS:
May cause cancer by inhalation.
Causes damage to lungs through prolonged or repeated exposure by inhalation.
* 0 0 E
Gerstley Borate
Amtalc-C98 Talc Harmful WARNING Causes mild skin irritation
Harmful if inhaled
May cause respiratory irritation
1 0 0 E
Dolomite Health Hazard DANGER May cause cancer (Inhalation) 1 0 0 E
EPK HarmfulHealth Hazard DANGER EPK Kaolin is a naturally occurring mineral, which may contain amounts of crystalline silica
typically 0.1-1.0%, may cause damage to respiratory system through prolonged or repeated
exposure.
1 0 0 E
Manganese Carbonate Health Hazard DANGER Causes damage to organs through prolonged or repeated exposure.
Cobalt Carbonate Health HazardEnvironmental Hazard DANGER May cause cancer
Suspected of causing genetic effects
May damage fertility or the unborn child
May cause allergy or breathing difficulties if inhaled
May cause a allergic skin reaction
Very toxic to aquatic life
Very toxic to aquatic life with long lasting effects
2 0 0 *
Bentonite Harmful WARNING Causes eye irritation
Causes skin irritation
May cause respiratory irritation