Cedar Hill Studio new Woo Yellow recipe.

Material Amount Batch Subtotal
Nepheline Syenite (Theoretical) 43
Strontium Carbonate 19
EPK 11
Frit 3124 10
Gerstley Borate 9
Dolomite 5
Silica 3
Total Base:100
Zircopax 15
Red iron oxide 4
Total: 119

Percentage Analysis

Ingredient Amount SiO2 Al2O3 B2O3 MgO CaO SrO K2O Na2O KNaO P2O5 Fe2O3 TiO2 ZrO2 LOI
Nepheline Syenite (Theoretical)4326.110.020.040.31.984.216.190.040.3
Strontium Carbonate1913.345.66
EPK115.034.110.010.020.040.010.050.030.080.041.63
Frit 3124105.530.991.381.410.070.630.7
Gerstley Borate91.330.092.410.311.750.040.360.40.010.040.012.66
Dolomite51.11.522.38
Silica33
Zircopax154.9210.08
Red iron oxide43.80.2
Total11945.9115.213.791.46513.342.125.217.330.043.960.0510.0812.83
100% no LOI 43.2414.323.571.384.7112.5624.916.90.043.730.059.5

Unity Molecular Formula (UMF)

FLUXES

RO/R2O

0.23 Na2O
0.06 K2O
0.36 SrO
0.25 CaO
0.1 MgO
STABILIZERS

R2O3

0.41 Al2O3
0.15 B2O3
GLASS-FORMERS

RO2

2.12 SiO2
0.23 ZrO2
OTHER

 

0.07 Fe2O3
SILICA:ALUMINA

SiO2:Al2O3

5.12

FLUX RATIO

R2O:RO

0.3 : 0.7

SiO2:Al2O3 Chart

Closest 100 neighbors in Glaze.

Click and drag to zoom
Stull Chart
SiO2:Al2O3 Ratio
SiO2:Al2O3 Ratio 5.12

Similar Base Recipes

No recipes with similar base ingredients and amounts were found.

Similar RO/R2O Unity Formulas

No recipes with similar RO/R2O Unity Formulas were found.

No reviews yet.

Hazards

09/2016 Note: This is a new feature. If a recipe material is not listed, that material's data has not yet been added. Some materials only have GHS ratings, while others only have HMIS ratings. Warnings differ between systems and countries. Glazy does not take any responsibility for accuracy of linked SDS information. Contact your ceramics supplier for safety information for your specific materials.
Globally Harmonized System (GHS) Hazardous Materials Identification System (HMIS) SDS Link
Material Pictograms Signal Word Hazard Statements Health Flammability Hazard Protection
Strontium Carbonate Harmful WARNING Product dust may be irritating to eyes,skin and respiratory system.  1 0 0 E
EPK HarmfulHealth Hazard DANGER EPK Kaolin is a naturally occurring mineral, which may contain amounts of crystalline silica
typically 0.1-1.0%, may cause damage to respiratory system through prolonged or repeated
exposure.
1 0 0 E
Gerstley Borate
Dolomite Health Hazard DANGER May cause cancer (Inhalation) 1 0 0 E
Silica HarmfulHealth Hazard DANGER From 200-Mesh SDS:
May cause cancer by inhalation.
Causes damage to lungs through prolonged or repeated exposure by inhalation.
* 0 0 E
Zircopax
Red iron oxide Health Hazard WARNING May cause damage to lung through prolonged or repeated exposure by inhalation