Category: Glaze > White, Off-White
Created 2017-10-01 22:58:50 by Allathea Joniec
Categories: Glaze > White, Off-White
Firing Temperature: Δ5-6
Atmospheres: Oxidation
Surface Type: Glossy

Material Amount Batch Subtotal
Soda Feldspar (Theoretical) 18
Frit 3134 18
Dolomite 18
Kaolin (Theoretical) 18
Silica 18
Spodumene (Theoretical) 10
Total Base:100
Tin Oxide 6.5
Zircopax 6.5
Bentonite 2
Red iron oxide 2
Total: 117

Percentage Analysis

Ingredient Amount SiO2 Al2O3 B2O3 MgO CaO Li2O K2O Na2O KNaO Fe2O3 ZrO2 SnO2 LOI
Soda Feldspar (Theoretical)1812.373.52.132.13
Frit 3134188.374.163.621.851.85
Dolomite183.945.498.57
Kaolin (Theoretical)188.517.242.25
Silica1818
Spodumene (Theoretical)106.462.740.8
Tin Oxide6.56.5
Zircopax6.52.134.37
Bentonite21.190.40.040.020.020.060.080.070.2
Red iron oxide21.90.1
Total11757.0313.884.163.989.130.80.024.044.061.974.376.511.12
100% no LOI 53.8613.113.933.768.620.760.023.813.831.864.136.14

Unity Molecular Formula (UMF)

FLUXES

RO/R2O

0.18 Na2O
0.08 Li2O
0.46 CaO
0.28 MgO
STABILIZERS

R2O3

0.38 Al2O3
0.17 B2O3
GLASS-FORMERS

RO2

2.68 SiO2
0.1 ZrO2
0.12 SnO2
OTHER

 

0.03 Fe2O3
SILICA:ALUMINA

SiO2:Al2O3

6.97

FLUX RATIO

R2O:RO

0.26 : 0.74

SiO2:Al2O3 Chart

Closest 100 neighbors in Glaze > White, Off-White.

Click and drag to zoom
Stull Chart
SiO2:Al2O3 Ratio
SiO2:Al2O3 Ratio 6.97

Similar RO/R2O Unity Formulas

R2O3 - STABILIZERS RO2 - GLASS FORMERS RO/R2O - FLUXES
Recipe Name ΔTemp Al2O3 B2O3 SiO2 ZrO2 SnO2 TiO2 KNaO K2O Na2O CaO MgO ZnO BaO PbO Li2O SrO
Folk Art Guild White- 3134 Sn6.5/Zr6.5 (variation) 5-6 0.38 0.17 2.68 0.1 0.12 0.18 0.18 0.46 0.28 0.08
Folk Art Guild White- 3134 Sn6.5/Zr6.5 5-6 0.38 0.17 2.68 0.1 0.12 0.18 0.18 0.46 0.28 0.08

No reviews yet.

Hazards

09/2016 Note: This is a new feature. If a recipe material is not listed, that material's data has not yet been added. Some materials only have GHS ratings, while others only have HMIS ratings. Warnings differ between systems and countries. Glazy does not take any responsibility for accuracy of linked SDS information. Contact your ceramics supplier for safety information for your specific materials.
Globally Harmonized System (GHS) Hazardous Materials Identification System (HMIS) SDS Link
Material Pictograms Signal Word Hazard Statements Health Flammability Hazard Protection
Dolomite Health Hazard DANGER May cause cancer (Inhalation) 1 0 0 E
Kaolin (Theoretical) HarmfulHealth Hazard DANGER SDS for EPK KAOLIN: EPK Kaolin is a naturally occurring mineral, which may contain amounts of crystalline silica
typically 0.1-1.0%, may cause damage to respiratory system through prolonged or repeated
exposure.
Silica HarmfulHealth Hazard DANGER From 200-Mesh SDS:
May cause cancer by inhalation.
Causes damage to lungs through prolonged or repeated exposure by inhalation.
* 0 0 E
Spodumene (Theoretical) Health Hazard DANGER May cause cancer by inhalation.
Causes damage to organs through prolonged or repeated exposure.
Tin Oxide Harmful WARNING Harmful if swallowed.
Zircopax
Bentonite Harmful WARNING Causes eye irritation
Causes skin irritation
May cause respiratory irritation
Red iron oxide Health Hazard WARNING May cause damage to lung through prolonged or repeated exposure by inhalation