Material Amount Batch Subtotal
Silica 34.15
Frit 3134 23.07
EPK 17.8
Neph Sye A270 16.62
Vansil W-30 Wollastonite 6.27
Amtalc-C98 Talc 2.09
Total: 100

Percentage Analysis

Ingredient Amount SiO2 Al2O3 B2O3 MgO CaO K2O Na2O KNaO P2O5 Fe2O3 TiO2 MnO LOI
Silica34.1534.15
Frit 313423.0710.735.334.642.372.37
EPK17.88.146.650.020.030.060.010.070.050.140.072.64
Neph Sye A27016.6210.013.920.060.811.732.540.010.08
Vansil W-30 Wollastonite6.273.140.040.092.820.010.010.010.010.1
Amtalc-C98 Talc2.091.120.010.620.070.010.010.010.25
Total10067.2810.625.330.737.640.874.124.990.050.170.070.013.07
100% no LOI 69.4410.965.50.767.880.94.255.150.050.180.070.01

Unity Molecular Formula (UMF)

FLUXES

RO/R2O

0.29 Na2O
0.04 K2O
0.59 CaO
0.08 MgO
STABILIZERS

R2O3

0.45 Al2O3
0.33 B2O3
GLASS-FORMERS

RO2

4.86 SiO2
SILICA:ALUMINA

SiO2:Al2O3

10.75

FLUX RATIO

R2O:RO

0.33 : 0.67

SiO2:Al2O3 Chart

Closest 100 neighbors in Glaze.

Click and drag to zoom
Stull Chart
SiO2:Al2O3 Ratio
SiO2:Al2O3 Ratio 10.75

Similar Base Recipes

No recipes with similar base ingredients and amounts were found.

Similar RO/R2O Unity Formulas

R2O3 - STABILIZERS RO2 - GLASS FORMERS RO/R2O - FLUXES
Recipe Name ΔTemp Al2O3 B2O3 SiO2 ZrO2 SnO2 TiO2 KNaO K2O Na2O CaO MgO ZnO BaO PbO Li2O SrO
Clear Gloss G2926B 6 0.45 0.33 4.86 0.33 0.04 0.29 0.59 0.08
Cone 6 Whiteware/Porcelain Transparent Base Glaze - Plainsman 6 0.45 0.33 4.89 0.32 0.04 0.28 0.61 0.08

No reviews yet.

Hazards

09/2016 Note: This is a new feature. If a recipe material is not listed, that material's data has not yet been added. Some materials only have GHS ratings, while others only have HMIS ratings. Warnings differ between systems and countries. Glazy does not take any responsibility for accuracy of linked SDS information. Contact your ceramics supplier for safety information for your specific materials.
Globally Harmonized System (GHS) Hazardous Materials Identification System (HMIS) SDS Link
Material Pictograms Signal Word Hazard Statements Health Flammability Hazard Protection
Silica HarmfulHealth Hazard DANGER From 200-Mesh SDS:
May cause cancer by inhalation.
Causes damage to lungs through prolonged or repeated exposure by inhalation.
* 0 0 E
EPK HarmfulHealth Hazard DANGER EPK Kaolin is a naturally occurring mineral, which may contain amounts of crystalline silica
typically 0.1-1.0%, may cause damage to respiratory system through prolonged or repeated
exposure.
1 0 0 E
Neph Sye A270
Vansil W-30 Wollastonite Health Hazard DANGER May cause cancer if inhaled.
Causes damage to organs through prolonged or repeated exposure if inhaled. (respiratory tract)
Amtalc-C98 Talc Harmful WARNING Causes mild skin irritation
Harmful if inhaled
May cause respiratory irritation
1 0 0 E