Category: Glaze > White, Off-White
Created 2017-10-09 08:50:46 by Triin Lehismets
Categories: Glaze > White, Off-White
Firing Temperature: Δ5-7
Atmospheres: Oxidation
Surface Type: Glossy
Transparency: Semi-opaque

Recipe from J. Britt mid-range glaze book p. 76

Material Amount Batch Subtotal
Nepheline Syenite Norwegian 38
Silica 25
Gerstley Borate 10
Zettlitzer kaolin 8
Whiting 7
Zinc Oxide 5
Talc (Theoretical) 5
Wollastonite (Theoretical) 2
Total Base:100
Rutile 8
Bentonite 2
Total: 110

Percentage Analysis

Ingredient Amount SiO2 Al2O3 B2O3 MgO CaO ZnO K2O Na2O KNaO P2O5 Fe2O3 TiO2 LOI
Nepheline Syenite Norwegian3822.228.813.262.876.130.080.76
Silica2525
Gerstley Borate101.480.12.680.351.940.040.40.440.010.040.012.95
Zettlitzer kaolin83.73.150.010.061.04
Whiting73.933.07
Zinc Oxide55
Talc (Theoretical)53.171.590.24
Wollastonite (Theoretical)21.030.97
Rutile80.797.20.01
Bentonite21.190.40.040.020.020.060.080.070.2
Total11057.7912.462.681.986.8653.323.336.650.011.047.218.27
100% no LOI 56.8312.262.641.956.754.923.263.286.540.011.027.09

Unity Molecular Formula (UMF)

FLUXES

RO/R2O

0.17 Na2O
0.11 K2O
0.19 ZnO
0.38 CaO
0.15 MgO
STABILIZERS

R2O3

0.38 Al2O3
0.12 B2O3
GLASS-FORMERS

RO2

2.99 SiO2
0.28 TiO2
OTHER

 

0.02 Fe2O3
SILICA:ALUMINA

SiO2:Al2O3

7.86

FLUX RATIO

R2O:RO

0.28 : 0.72

SiO2:Al2O3 Chart

Closest 100 neighbors in Glaze > White, Off-White.

Click and drag to zoom
Stull Chart
SiO2:Al2O3 Ratio
SiO2:Al2O3 Ratio 7.86

Similar Base Recipes

No recipes with similar base ingredients and amounts were found.

Similar RO/R2O Unity Formulas

No recipes with similar RO/R2O Unity Formulas were found.

No reviews yet.

Hazards

09/2016 Note: This is a new feature. If a recipe material is not listed, that material's data has not yet been added. Some materials only have GHS ratings, while others only have HMIS ratings. Warnings differ between systems and countries. Glazy does not take any responsibility for accuracy of linked SDS information. Contact your ceramics supplier for safety information for your specific materials.
Globally Harmonized System (GHS) Hazardous Materials Identification System (HMIS) SDS Link
Material Pictograms Signal Word Hazard Statements Health Flammability Hazard Protection
Silica HarmfulHealth Hazard DANGER From 200-Mesh SDS:
May cause cancer by inhalation.
Causes damage to lungs through prolonged or repeated exposure by inhalation.
* 0 0 E
Gerstley Borate
Whiting Harmful WARNING Causes eye irritation
Zinc Oxide 0 0 0 *
Talc (Theoretical) Harmful WARNING Causes mild skin irritation
Harmful if inhaled
May cause respiratory irritation
1 0 0 E
Wollastonite (Theoretical) Health Hazard DANGER Vansil W-30 Wollastonite SDS:
May cause cancer if inhaled.
Causes damage to organs through prolonged or repeated exposure if inhaled. (respiratory tract)
Rutile 1 0 0
Bentonite Harmful WARNING Causes eye irritation
Causes skin irritation
May cause respiratory irritation