Material Amount Batch Subtotal
Custer Feldspar 31.68
Silica 28.71
Whiting 18.81
EPK 8.91
Talc (Theoretical) 6.93
Titanium Dioxide 2.97
Bone Ash 1.98
Total: 99.99

Percentage Analysis

Ingredient Amount SiO2 Al2O3 MgO CaO K2O Na2O KNaO P2O5 Fe2O3 TiO2 LOI
Custer Feldspar31.6821.75.390.13.170.954.120.030.1
Silica28.7128.71
Whiting18.8110.558.26
EPK8.914.073.330.010.020.030.010.040.020.070.031.32
Talc (Theoretical)6.934.392.210.33
Titanium Dioxide2.972.97
Bone Ash1.981.110.840.04
Total99.9958.888.712.2211.773.20.964.160.860.1310.04
100%58.888.722.2211.773.20.964.160.860.1310.04
100% no LOI 65.649.722.4713.123.571.074.630.960.113.35

Unity Molecular Formula (UMF)

FLUXES

RO/R2O

0.05 Na2O
0.11 K2O
0.67 CaO
0.17 MgO
STABILIZERS

R2O3

0.27 Al2O3
GLASS-FORMERS

RO2

3.12 SiO2
0.12 TiO2
OTHER

 

0.02 P2O5
SILICA:ALUMINA

SiO2:Al2O3

11.44

FLUX RATIO

R2O:RO

0.16 : 0.84

SiO2:Al2O3 Chart

Closest 100 neighbors in Glaze > White, Off-White.

Click and drag to zoom
Stull Chart
SiO2:Al2O3 Ratio
SiO2:Al2O3 Ratio 11.44

Similar Base Recipes

No recipes with similar base ingredients and amounts were found.

Similar RO/R2O Unity Formulas

No recipes with similar RO/R2O Unity Formulas were found.

No reviews yet.

Hazards

09/2016 Note: This is a new feature. If a recipe material is not listed, that material's data has not yet been added. Some materials only have GHS ratings, while others only have HMIS ratings. Warnings differ between systems and countries. Glazy does not take any responsibility for accuracy of linked SDS information. Contact your ceramics supplier for safety information for your specific materials.
Globally Harmonized System (GHS) Hazardous Materials Identification System (HMIS) SDS Link
Material Pictograms Signal Word Hazard Statements Health Flammability Hazard Protection
Custer Feldspar HarmfulHealth Hazard WARNING May cause damage to lungs through prolonged or repeated inhalation.
Suspected of causing cancer through
prolonged or repeated inhalation.
May cause allergy or asthma symptoms or breathing difficulties if inhaled.
May cause skin or eye irritation.
Silica HarmfulHealth Hazard DANGER From 200-Mesh SDS:
May cause cancer by inhalation.
Causes damage to lungs through prolonged or repeated exposure by inhalation.
* 0 0 E
Whiting Harmful WARNING Causes eye irritation
EPK HarmfulHealth Hazard DANGER EPK Kaolin is a naturally occurring mineral, which may contain amounts of crystalline silica
typically 0.1-1.0%, may cause damage to respiratory system through prolonged or repeated
exposure.
1 0 0 E
Talc (Theoretical) Harmful WARNING Causes mild skin irritation
Harmful if inhaled
May cause respiratory irritation
1 0 0 E
Titanium Dioxide Health Hazard WARNING Suspected of causing cancer
Bone Ash