Category: Glaze
Created 2017-11-04 21:19:45 by IU Southeast Ceramics
Categories: Glaze
Firing Temperature: Δ10
Atmospheres: Reduction
Surface Type: Satin - Matte
Transparency: Opaque

Material Amount Batch Subtotal
Minspar 200 51
EPK 17.1
Dolomite 15.6
Silica 10.6
Magnesium carbonate 5.7
Total Base:100
Zircopax 1
Total: 101

Percentage Analysis

Ingredient Amount SiO2 Al2O3 MgO CaO K2O Na2O KNaO P2O5 Fe2O3 TiO2 ZrO2 LOI
Minspar 2005135.149.480.772.13.335.430.030.15
EPK17.17.826.390.020.030.060.010.070.040.130.072.53
Dolomite15.63.424.767.43
Silica10.610.6
Magnesium carbonate5.72.722.98
Zircopax10.330.67
Total10153.8915.876.165.562.163.345.50.040.160.070.6713.09
100% no LOI 61.318.057.016.322.463.86.260.050.180.070.76

Unity Molecular Formula (UMF)

FLUXES

RO/R2O

0.16 Na2O
0.07 K2O
0.3 CaO
0.46 MgO
STABILIZERS

R2O3

0.47 Al2O3
GLASS-FORMERS

RO2

2.73 SiO2
0.02 ZrO2
SILICA:ALUMINA

SiO2:Al2O3

5.76

FLUX RATIO

R2O:RO

0.23 : 0.77

SiO2:Al2O3 Chart

Closest 100 neighbors in Glaze.

Click and drag to zoom
Stull Chart
SiO2:Al2O3 Ratio
SiO2:Al2O3 Ratio 5.76

Similar Base Recipes

Similar RO/R2O Unity Formulas

No recipes with similar RO/R2O Unity Formulas were found.

No reviews yet.

Hazards

09/2016 Note: This is a new feature. If a recipe material is not listed, that material's data has not yet been added. Some materials only have GHS ratings, while others only have HMIS ratings. Warnings differ between systems and countries. Glazy does not take any responsibility for accuracy of linked SDS information. Contact your ceramics supplier for safety information for your specific materials.
Globally Harmonized System (GHS) Hazardous Materials Identification System (HMIS) SDS Link
Material Pictograms Signal Word Hazard Statements Health Flammability Hazard Protection
Minspar 200 Health Hazard WARNING May cause damage to lung through prolonged or repeated inhalation 2 0 0 E
EPK HarmfulHealth Hazard DANGER EPK Kaolin is a naturally occurring mineral, which may contain amounts of crystalline silica
typically 0.1-1.0%, may cause damage to respiratory system through prolonged or repeated
exposure.
1 0 0 E
Dolomite Health Hazard DANGER May cause cancer (Inhalation) 1 0 0 E
Silica HarmfulHealth Hazard DANGER From 200-Mesh SDS:
May cause cancer by inhalation.
Causes damage to lungs through prolonged or repeated exposure by inhalation.
* 0 0 E
Magnesium carbonate WARNING Causes mild skin irritation
Causes eye irritation
Zircopax