Category: Glaze > Raku
Created 2017-11-06 21:20:46 by IU Southeast Ceramics
Categories: Glaze > Raku
Firing Temperature: Δ06-04
Atmospheres: Raku
Surface Type: Glossy - Semi

Material Amount Batch Subtotal
Frit 3134 50
Gillespie Borate 50
Total Base:100
Tin Oxide 3
Copper Oxide 2.5
Total: 105.5

Percentage Analysis

Ingredient Amount SiO2 Al2O3 B2O3 MgO CaO SrO Na2O KNaO CuO SnO2 LOI
Frit 31345023.2511.5410.065.145.14
Gillespie Borate505.90.8512.251.9511.50.231.881.8815.45
Tin Oxide33
Copper Oxide2.52.5
Total105.529.150.8523.791.9521.560.237.027.022.5315.45
100% no LOI 32.370.9426.422.1623.940.257.87.82.783.33

Unity Molecular Formula (UMF)

FLUXES

RO/R2O

0.21 Na2O
0.7 CaO
0.09 MgO
STABILIZERS

R2O3

0.02 Al2O3
0.62 B2O3
GLASS-FORMERS

RO2

0.88 SiO2
0.04 SnO2
OTHER

 

0.06 CuO
SILICA:ALUMINA

SiO2:Al2O3

58.30

FLUX RATIO

R2O:RO

0.21 : 0.79

SiO2:Al2O3 Chart

Closest 63 neighbors in Glaze > Raku.

Click and drag to zoom
Stull Chart
SiO2:Al2O3 Ratio
SiO2:Al2O3 Ratio 58.3

Similar Base Recipes

No recipes with similar base ingredients and amounts were found.

Similar RO/R2O Unity Formulas

No recipes with similar RO/R2O Unity Formulas were found.

No reviews yet.

Hazards

09/2016 Note: This is a new feature. If a recipe material is not listed, that material's data has not yet been added. Some materials only have GHS ratings, while others only have HMIS ratings. Warnings differ between systems and countries. Glazy does not take any responsibility for accuracy of linked SDS information. Contact your ceramics supplier for safety information for your specific materials.
Globally Harmonized System (GHS) Hazardous Materials Identification System (HMIS) SDS Link
Material Pictograms Signal Word Hazard Statements Health Flammability Hazard Protection
Tin Oxide Harmful WARNING Harmful if swallowed.
Copper Oxide Harmful WARNING Harmful if swallowed 2 0 0 E