Category: Glaze
Created 2017-11-09 20:46:50 by Ginger Lukas
Categories: Glaze
Firing Temperature: Δ6
Atmospheres: Oxidation
Surface Type: Glossy
Transparency: Transparent

acid green and runny as hell but so worth it

Material Amount Batch Subtotal
Nepheline Syenite (Theoretical) 46
Gerstley Borate 12
Whiting 12
Silica 12
EPK 12
Lithium Carbonate 6
Chrome Oxide 0.5
Total: 100.5

Percentage Analysis

Ingredient Amount SiO2 Al2O3 B2O3 MgO CaO Li2O K2O Na2O KNaO P2O5 Fe2O3 TiO2 Cr2O3 LOI
Nepheline Syenite (Theoretical)4627.9210.720.050.322.124.516.630.050.32
Gerstley Borate121.780.123.220.422.330.050.480.530.010.050.013.54
Whiting126.735.27
Silica1212
EPK125.494.480.010.020.040.010.050.030.090.051.78
Lithium Carbonate62.443.56
Chrome Oxide0.50.5
Total100.547.1915.323.220.489.42.442.2157.20.040.180.060.514.46
100% no LOI 54.8417.813.740.5610.932.842.565.818.370.050.210.070.58

Unity Molecular Formula (UMF)

FLUXES

RO/R2O

0.22 Na2O
0.06 K2O
0.22 Li2O
0.46 CaO
0.03 MgO
STABILIZERS

R2O3

0.41 Al2O3
0.13 B2O3
GLASS-FORMERS

RO2

2.15 SiO2
OTHER

 

0.01 Cr2O3
SILICA:ALUMINA

SiO2:Al2O3

5.23

FLUX RATIO

R2O:RO

0.51 : 0.49

SiO2:Al2O3 Chart

Closest 100 neighbors in Glaze.

Click and drag to zoom
Stull Chart
SiO2:Al2O3 Ratio
SiO2:Al2O3 Ratio 5.23

Similar Base Recipes

No recipes with similar base ingredients and amounts were found.

Similar RO/R2O Unity Formulas

No recipes with similar RO/R2O Unity Formulas were found.

No reviews yet.

Hazards

09/2016 Note: This is a new feature. If a recipe material is not listed, that material's data has not yet been added. Some materials only have GHS ratings, while others only have HMIS ratings. Warnings differ between systems and countries. Glazy does not take any responsibility for accuracy of linked SDS information. Contact your ceramics supplier for safety information for your specific materials.
Globally Harmonized System (GHS) Hazardous Materials Identification System (HMIS) SDS Link
Material Pictograms Signal Word Hazard Statements Health Flammability Hazard Protection
Gerstley Borate
Whiting Harmful WARNING Causes eye irritation
Silica HarmfulHealth Hazard DANGER From 200-Mesh SDS:
May cause cancer by inhalation.
Causes damage to lungs through prolonged or repeated exposure by inhalation.
* 0 0 E
EPK HarmfulHealth Hazard DANGER EPK Kaolin is a naturally occurring mineral, which may contain amounts of crystalline silica
typically 0.1-1.0%, may cause damage to respiratory system through prolonged or repeated
exposure.
1 0 0 E
Lithium Carbonate Harmful WARNING Harmful if swallowed.
Causes serious eye irritation.
Harmful to aquatic life.
Chrome Oxide WARNING May be harmful if inhaled. May cause
irritation to eyes and respiratory tract. Slightly toxic if ingested.
2 0 1 E