Category: Glaze
Created 2017-11-29 14:24:15 by Clemson University---Ceramic Dept.
Categories: Glaze
Firing Temperature: Δ05-04
Atmospheres: Oxidation
Surface Type: Satin - Matte

Hirsch Satin Matte Yellow glaze for introduction to ceramics ART 2170

Material Amount Batch Subtotal
Silica 35
Gerstley Borate 32
Whiting 17
Lithium Carbonate 9
Neph Sye A270 4
EPK 4
Bentonite 2
Total Base:103
Mason Stain 6410 Canary 7
Total: 110

Percentage Analysis

Ingredient Amount SiO2 Al2O3 B2O3 MgO CaO Li2O K2O Na2O KNaO P2O5 Fe2O3 TiO2 LOI
Silica3535
Gerstley Borate324.740.328.581.126.210.131.281.410.030.130.039.44
Whiting179.547.46
Lithium Carbonate93.675.33
Neph Sye A27042.410.940.020.190.420.610.02
EPK41.831.490.010.010.010.010.030.020.59
Bentonite21.190.40.040.020.020.060.080.070.2
Mason Stain 6410 Canary7
Total11045.163.168.581.1615.793.670.361.762.120.040.230.0523.05
100% no LOI 56.483.9510.731.4619.754.590.452.22.650.050.290.06

Unity Molecular Formula (UMF)

FLUXES

RO/R2O

0.06 Na2O
0.01 K2O
0.26 Li2O
0.61 CaO
0.06 MgO
STABILIZERS

R2O3

0.07 Al2O3
0.26 B2O3
GLASS-FORMERS

RO2

1.62 SiO2
SILICA:ALUMINA

SiO2:Al2O3

24.24

FLUX RATIO

R2O:RO

0.33 : 0.67

SiO2:Al2O3 Chart

Closest 100 neighbors in Glaze.

Click and drag to zoom
Stull Chart
SiO2:Al2O3 Ratio
SiO2:Al2O3 Ratio 24.24

Similar RO/R2O Unity Formulas

R2O3 - STABILIZERS RO2 - GLASS FORMERS RO/R2O - FLUXES
Recipe Name ΔTemp Al2O3 B2O3 SiO2 ZrO2 SnO2 TiO2 KNaO K2O Na2O CaO MgO ZnO BaO PbO Li2O SrO
Hirsch Satin Matte Yellow Cone--04 Glaze 05-04 0.07 0.26 1.62 0.07 0.01 0.06 0.61 0.06 0.26
Hirsh Satin Matt Base Glaze 04-02 0.07 0.26 1.62 0.07 0.01 0.06 0.61 0.06 0.26
Hirsch Satin Matte Cone--04 Glaze Base 05-04 0.07 0.26 1.62 0.07 0.01 0.06 0.61 0.06 0.26
Hirsch Satin Matte Green Cone--04 Glaze 05-04 0.07 0.26 1.62 0.07 0.01 0.06 0.61 0.06 0.26
Hirsch Satin Matte Turquoise Cone--04 Glaze 05-04 0.07 0.26 1.62 0.07 0.01 0.06 0.61 0.06 0.26
Hirsch Satin Matte Rose Cone--04 Glaze 05-04 0.07 0.26 1.62 0.07 0.01 0.06 0.61 0.06 0.26
Hirsch Satin Matte Orange Cone--04 Glaze 05-04 0.07 0.26 1.62 0.07 0.01 0.06 0.61 0.06 0.26
Hirsch Satin Matte Mint Cone--04 Glaze 05-04 0.07 0.26 1.62 0.07 0.01 0.06 0.61 0.06 0.26
Hirsch Satin Matte Purple Cone--04 Glaze 05-04 0.07 0.26 1.62 0.07 0.01 0.06 0.61 0.06 0.26

No reviews yet.

Hazards

09/2016 Note: This is a new feature. If a recipe material is not listed, that material's data has not yet been added. Some materials only have GHS ratings, while others only have HMIS ratings. Warnings differ between systems and countries. Glazy does not take any responsibility for accuracy of linked SDS information. Contact your ceramics supplier for safety information for your specific materials.
Globally Harmonized System (GHS) Hazardous Materials Identification System (HMIS) SDS Link
Material Pictograms Signal Word Hazard Statements Health Flammability Hazard Protection
Silica HarmfulHealth Hazard DANGER From 200-Mesh SDS:
May cause cancer by inhalation.
Causes damage to lungs through prolonged or repeated exposure by inhalation.
* 0 0 E
Gerstley Borate
Whiting Harmful WARNING Causes eye irritation
Lithium Carbonate Harmful WARNING Harmful if swallowed.
Causes serious eye irritation.
Harmful to aquatic life.
Neph Sye A270
EPK HarmfulHealth Hazard DANGER EPK Kaolin is a naturally occurring mineral, which may contain amounts of crystalline silica
typically 0.1-1.0%, may cause damage to respiratory system through prolonged or repeated
exposure.
1 0 0 E
Bentonite Harmful WARNING Causes eye irritation
Causes skin irritation
May cause respiratory irritation