Category: Glaze > Green
Created 1996-06-02 09:00:00 by Glazy Admin
Categories: Glaze > Green
Firing Temperature: Δ5-7
Atmospheres: Oxidation

Glaze Type: Mid-fire

It is between a lime and chartreuse.
submitted by: Beth Fusaro e-mail:

Material Amount Batch Subtotal
Nepheline Syenite (Theoretical) 46.7
Silica 25
Gerstley Borate 10.9
Dolomite 10.9
Ball Clay (Theoretical) 6.5
Total Base:100
Titanium Dioxide 7.6
Copper Carbonate 1.6
Bentonite 1.1
Total: 110.3

Percentage Analysis

Ingredient Amount SiO2 Al2O3 B2O3 MgO CaO K2O Na2O KNaO P2O5 Fe2O3 TiO2 CuO LOI
Nepheline Syenite (Theoretical)46.728.3510.880.050.332.154.586.730.050.33
Silica2525
Gerstley Borate10.91.610.112.920.382.110.040.440.480.010.040.013.22
Dolomite10.92.393.325.19
Ball Clay (Theoretical)6.53.841.630.020.020.060.030.090.070.060.78
Titanium Dioxide7.67.6
Copper Carbonate1.61.030.57
Bentonite1.10.650.220.020.010.010.030.040.040.11
Total110.359.4512.842.922.865.792.265.077.330.010.197.681.0310.19
100% no LOI 59.3912.822.922.855.792.265.077.330.010.197.671.03

Unity Molecular Formula (UMF)

FLUXES

RO/R2O

0.29 Na2O
0.09 K2O
0.37 CaO
0.25 MgO
STABILIZERS

R2O3

0.45 Al2O3
0.15 B2O3
GLASS-FORMERS

RO2

3.53 SiO2
0.34 TiO2
OTHER

 

0.05 CuO
SILICA:ALUMINA

SiO2:Al2O3

7.86

FLUX RATIO

R2O:RO

0.38 : 0.62

SiO2:Al2O3 Chart

Closest 100 neighbors in Glaze > Green.

Click and drag to zoom
Stull Chart
SiO2:Al2O3 Ratio
SiO2:Al2O3 Ratio 7.86

Similar Base Recipes

No recipes with similar base ingredients and amounts were found.

Similar RO/R2O Unity Formulas

No recipes with similar RO/R2O Unity Formulas were found.

No reviews yet.

Hazards

09/2016 Note: This is a new feature. If a recipe material is not listed, that material's data has not yet been added. Some materials only have GHS ratings, while others only have HMIS ratings. Warnings differ between systems and countries. Glazy does not take any responsibility for accuracy of linked SDS information. Contact your ceramics supplier for safety information for your specific materials.
Globally Harmonized System (GHS) Hazardous Materials Identification System (HMIS) SDS Link
Material Pictograms Signal Word Hazard Statements Health Flammability Hazard Protection
Silica HarmfulHealth Hazard DANGER From 200-Mesh SDS:
May cause cancer by inhalation.
Causes damage to lungs through prolonged or repeated exposure by inhalation.
* 0 0 E
Gerstley Borate
Dolomite Health Hazard DANGER May cause cancer (Inhalation) 1 0 0 E
Titanium Dioxide Health Hazard WARNING Suspected of causing cancer
Copper Carbonate Harmful WARNING Harmful if swallowed.
Causes skin irritation.
Causes serious eye irritation.
Bentonite Harmful WARNING Causes eye irritation
Causes skin irritation