Category: Glaze
Created 2017-11-29 17:39:14 by Clemson University---Ceramic Dept.
Categories: Glaze
Firing Temperature: Δ9-10
Atmospheres: Oxidation, Reduction, Salt & Soda, Wood
Surface Type: Satin

Sam Chung Satin High Fire Glaze Base

Material Amount Batch Subtotal
Kona F-4 feldspar 35.7
Neph Sye A270 21.4
Calcined Kaolin 14.4
Whiting 14.3
Barium Carbonate 7.1
Zinc Oxide 7.1
Total Base:100
Copper Carbonate 0.5
Total: 100.5

Percentage Analysis

Ingredient Amount SiO2 Al2O3 MgO CaO BaO ZnO K2O Na2O KNaO Fe2O3 CuO LOI
Kona F-4 feldspar35.723.836.990.020.611.712.464.170.010.07
Neph Sye A27021.412.885.050.081.042.233.270.020.11
Calcined Kaolin14.47.796.61
Whiting14.38.026.28
Barium Carbonate7.15.511.59
Zinc Oxide7.17.1
Copper Carbonate0.50.320.18
Total100.544.518.650.028.715.517.12.754.697.440.030.328.22
100% no LOI 48.2220.210.029.445.977.692.985.088.060.030.35

Unity Molecular Formula (UMF)

FLUXES

RO/R2O

0.2 Na2O
0.08 K2O
0.09 BaO
0.23 ZnO
0.4 CaO
STABILIZERS

R2O3

0.48 Al2O3
GLASS-FORMERS

RO2

1.93 SiO2
OTHER

 

0.01 CuO
SILICA:ALUMINA

SiO2:Al2O3

4.05

FLUX RATIO

R2O:RO

0.27 : 0.73

SiO2:Al2O3 Chart

Closest 100 neighbors in Glaze.

Click and drag to zoom
Stull Chart
SiO2:Al2O3 Ratio
SiO2:Al2O3 Ratio 4.05

Similar Base Recipes

No recipes with similar base ingredients and amounts were found.

Similar RO/R2O Unity Formulas

No recipes with similar RO/R2O Unity Formulas were found.

No reviews yet.

Hazards

09/2016 Note: This is a new feature. If a recipe material is not listed, that material's data has not yet been added. Some materials only have GHS ratings, while others only have HMIS ratings. Warnings differ between systems and countries. Glazy does not take any responsibility for accuracy of linked SDS information. Contact your ceramics supplier for safety information for your specific materials.
Globally Harmonized System (GHS) Hazardous Materials Identification System (HMIS) SDS Link
Material Pictograms Signal Word Hazard Statements Health Flammability Hazard Protection
Neph Sye A270
Whiting Harmful WARNING Causes eye irritation
Barium Carbonate Harmful WARNING Harmful if swallowed. 2 0 1 *
Zinc Oxide 0 0 0 *
Copper Carbonate Harmful WARNING Harmful if swallowed.
Causes skin irritation.
Causes serious eye irritation.