Category: Glaze > Green > Oribe
Created 2017-12-06 05:44:59 by Sid Henderson
Categories: Glaze > Green > Oribe
Firing Temperature: Δ9-10
Atmospheres: Oxidation, Neutral, Reduction
Surface Type: Glossy
Transparency: Translucent

Easily my favorite Oribe recipe, exhibiting bright green colors ranging from a lime green through to a turquoise blue. It can also exhibit metallic luster when really thick, although this glaze also tends to be pretty runny.

Material Amount Batch Subtotal
Custer Feldspar 31
Silica 25.3
Whiting 22.4
EPK 12.5
Talc (Theoretical) 7.8
Bone Ash 1
Total Base:100
Copper Oxide 5.5
Bentonite 2
Total: 107.5

Percentage Analysis

Ingredient Amount SiO2 Al2O3 MgO CaO K2O Na2O KNaO P2O5 Fe2O3 TiO2 CuO LOI
Custer Feldspar3121.245.270.093.10.934.030.030.09
Silica25.325.3
Whiting22.412.579.83
EPK12.55.724.670.010.020.040.010.050.030.10.051.85
Talc (Theoretical)7.84.942.490.37
Bone Ash10.560.420.02
Copper Oxide5.55.5
Bentonite21.190.40.040.020.020.060.080.070.2
Total107.558.3810.342.5413.263.1614.160.460.20.055.512.37
100% no LOI 61.5310.92.6813.983.331.054.390.480.210.055.8

Unity Molecular Formula (UMF)

FLUXES

RO/R2O

0.05 Na2O
0.1 K2O
0.68 CaO
0.18 MgO
STABILIZERS

R2O3

0.29 Al2O3
GLASS-FORMERS

RO2

2.79 SiO2
OTHER

 

0.01 P2O5
0.2 CuO
SILICA:ALUMINA

SiO2:Al2O3

9.57

FLUX RATIO

R2O:RO

0.14 : 0.86

SiO2:Al2O3 Chart

Closest 21 neighbors in Glaze > Green > Oribe.

Click and drag to zoom
Stull Chart
SiO2:Al2O3 Ratio
SiO2:Al2O3 Ratio 9.57

Similar RO/R2O Unity Formulas

R2O3 - STABILIZERS RO2 - GLASS FORMERS RO/R2O - FLUXES
Recipe Name ΔTemp Al2O3 B2O3 SiO2 ZrO2 SnO2 TiO2 KNaO K2O Na2O CaO MgO ZnO BaO PbO Li2O SrO
Shaner's Oribe 9-10 0.29 2.79 0.15 0.1 0.05 0.68 0.18
Raspberry Red to Pale Seagreen 10 0.28 2.75 0.14 0.1 0.04 0.68 0.18
Oribe 10 0.31 2.75 0.17 0.17 0.66 0.18
Shaner Oribe 10-11 0.29 2.75 0.14 0.1 0.04 0.68 0.18
Shaner's Oribe High Fire Glaze Base 9-10 0.29 2.75 0.15 0.1 0.05 0.69 0.17
Green Moss 10 0.29 2.76 0.14 0.1 0.04 0.68 0.18
Green Oribe 3 10 0.31 2.76 0.17 0.17 0.66 0.18
Shaner Oribe 10-11 0.29 2.77 0.15 0.1 0.05 0.68 0.18

No reviews yet.

Hazards

09/2016 Note: This is a new feature. If a recipe material is not listed, that material's data has not yet been added. Some materials only have GHS ratings, while others only have HMIS ratings. Warnings differ between systems and countries. Glazy does not take any responsibility for accuracy of linked SDS information. Contact your ceramics supplier for safety information for your specific materials.
Globally Harmonized System (GHS) Hazardous Materials Identification System (HMIS) SDS Link
Material Pictograms Signal Word Hazard Statements Health Flammability Hazard Protection
Custer Feldspar HarmfulHealth Hazard WARNING May cause damage to lungs through prolonged or repeated inhalation.
Suspected of causing cancer through
prolonged or repeated inhalation.
May cause allergy or asthma symptoms or breathing difficulties if inhaled.
May cause skin or eye irritation.
Silica HarmfulHealth Hazard DANGER From 200-Mesh SDS:
May cause cancer by inhalation.
Causes damage to lungs through prolonged or repeated exposure by inhalation.
* 0 0 E
Whiting Harmful WARNING Causes eye irritation
EPK HarmfulHealth Hazard DANGER EPK Kaolin is a naturally occurring mineral, which may contain amounts of crystalline silica
typically 0.1-1.0%, may cause damage to respiratory system through prolonged or repeated
exposure.
1 0 0 E
Talc (Theoretical) Harmful WARNING Causes mild skin irritation
Harmful if inhaled
May cause respiratory irritation
1 0 0 E
Bone Ash
Copper Oxide Harmful WARNING Harmful if swallowed 2 0 0 E
Bentonite Harmful WARNING Causes eye irritation
Causes skin irritation
May cause respiratory irritation