Category: Glaze > Red > Pink
Created 1995-04-10 09:00:00 by Glazy Admin
Categories: Glaze > Red > Pink
Firing Temperature: Δ6-7
Atmospheres: Oxidation
Surface Type: Satin - Matte
Transparency: Opaque

Glaze Type: Lithium Matt

Semi matt mauve, nice. From Brian Kemp, via
Rose Downs on ClayArt listserv. CLAY COLOR/TYPE: Buff Stoneware Fired
at 100 degrees per hour to 600 degrees, then free for all to cone
6-7. Kiln Size, Cromarty 25 cu ft. Manufactured in the UK.
CONTRIBUTOR: Brian Kemp, Nanyang Technological University, Block B,
Room 216, 469 Bukut Timah Rd., Singapore, 1025 TEST SITE: Nanyang
Technological University, Singapore

Material Amount Batch Subtotal
Nepheline Syenite (Theoretical) 43.3
Whiting 20
Lithium Carbonate 16.7
Gerstley Borate 8.3
Silica 6.7
Barium Carbonate 5
Total Base:100
Tin Oxide 8.3
Chrome Oxide 0.4
Total: 108.7

Percentage Analysis

Ingredient Amount SiO2 Al2O3 B2O3 MgO CaO BaO Li2O K2O Na2O KNaO P2O5 Fe2O3 TiO2 Cr2O3 SnO2 LOI
Nepheline Syenite (Theoretical)43.326.2810.090.040.31.994.246.230.040.3
Whiting2011.228.78
Lithium Carbonate16.76.89.9
Gerstley Borate8.31.230.082.220.291.610.030.330.360.010.030.012.45
Silica6.76.7
Barium Carbonate53.881.12
Tin Oxide8.38.3
Chrome Oxide0.40.4
Total108.734.2110.172.220.3313.133.886.82.034.586.60.010.080.010.48.322.55
100% no LOI 39.7111.812.580.3915.244.517.92.355.317.660.010.090.010.469.63

Unity Molecular Formula (UMF)

FLUXES

RO/R2O

0.12 Na2O
0.04 K2O
0.39 Li2O
0.04 BaO
0.4 CaO
0.01 MgO
STABILIZERS

R2O3

0.17 Al2O3
0.05 B2O3
GLASS-FORMERS

RO2

0.96 SiO2
0.09 SnO2
SILICA:ALUMINA

SiO2:Al2O3

5.71

FLUX RATIO

R2O:RO

0.55 : 0.45

SiO2:Al2O3 Chart

Closest 28 neighbors in Glaze > Red > Pink.

Click and drag to zoom
Stull Chart
SiO2:Al2O3 Ratio
SiO2:Al2O3 Ratio 5.71

Similar Base Recipes

No recipes with similar base ingredients and amounts were found.

Similar RO/R2O Unity Formulas

No recipes with similar RO/R2O Unity Formulas were found.

No reviews yet.

Hazards

09/2016 Note: This is a new feature. If a recipe material is not listed, that material's data has not yet been added. Some materials only have GHS ratings, while others only have HMIS ratings. Warnings differ between systems and countries. Glazy does not take any responsibility for accuracy of linked SDS information. Contact your ceramics supplier for safety information for your specific materials.
Globally Harmonized System (GHS) Hazardous Materials Identification System (HMIS) SDS Link
Material Pictograms Signal Word Hazard Statements Health Flammability Hazard Protection
Whiting Harmful WARNING Causes eye irritation
Lithium Carbonate Harmful WARNING Harmful if swallowed.
Causes serious eye irritation.
Harmful to aquatic life.
Gerstley Borate
Silica HarmfulHealth Hazard DANGER From 200-Mesh SDS:
May cause cancer by inhalation.
Causes damage to lungs through prolonged or repeated exposure by inhalation.
* 0 0 E
Barium Carbonate Harmful WARNING Harmful if swallowed. 2 0 1 *
Tin Oxide Harmful WARNING Harmful if swallowed.
Chrome Oxide WARNING May be harmful if inhaled. May cause
irritation to eyes and respiratory tract. Slightly toxic if ingested.
2 0 1 E