Category: Glaze > Red > Pink
Created 1995-07-18 09:00:00 by Glazy Admin
Categories: Glaze > Red > Pink
Firing Temperature: Δ6
Atmospheres: Oxidation
Surface Type: Matte
Transparency: Opaque

Glaze Type: Mid-fire

Here's a neat plum glaze, rather misnamed 'Nickel Pink.' It's 6^ ox.
and comes from Emanual Coopers recipe file. Was printed in Ceramic
Review May/June/87. When it is applied rather thickly, it is a
beautiful rich plum color, breaking on the edges to a leather brown.
submitted by: Dan Taylor e-mail:

Material Amount Batch Subtotal
Barium Carbonate 41.67
Nepheline Syenite (Theoretical) 26.04
Silica 16.67
Zinc Oxide 12.5
Lithium Carbonate 3.12
Total Base:100
Bentonite 4.17
Nickel Oxide 1.56
Total: 105.73

Percentage Analysis

Ingredient Amount SiO2 Al2O3 MgO CaO BaO ZnO Li2O K2O Na2O KNaO Fe2O3 NiO LOI
Barium Carbonate41.6732.369.31
Nepheline Syenite (Theoretical)26.0415.816.070.030.181.22.553.750.030.18
Silica16.6716.67
Zinc Oxide12.512.5
Lithium Carbonate3.121.271.85
Bentonite4.172.470.840.080.040.040.130.170.150.42
Nickel Oxide1.561.56
Total105.7334.956.910.110.2232.3612.51.271.242.683.920.171.5611.76
100% no LOI 37.197.350.120.2434.4413.31.351.322.854.170.181.66

Unity Molecular Formula (UMF)

FLUXES

RO/R2O

0.09 Na2O
0.03 K2O
0.09 Li2O
0.45 BaO
0.33 ZnO
0.01 CaO
0.01 MgO
STABILIZERS

R2O3

0.14 Al2O3
GLASS-FORMERS

RO2

1.24 SiO2
OTHER

 

0.04 NiO
SILICA:ALUMINA

SiO2:Al2O3

8.59

FLUX RATIO

R2O:RO

0.21 : 0.79

SiO2:Al2O3 Chart

Closest 28 neighbors in Glaze > Red > Pink.

Click and drag to zoom
Stull Chart
SiO2:Al2O3 Ratio
SiO2:Al2O3 Ratio 8.59

Similar Base Recipes

Δ6

Similar RO/R2O Unity Formulas

R2O3 - STABILIZERS RO2 - GLASS FORMERS RO/R2O - FLUXES
Recipe Name ΔTemp Al2O3 B2O3 SiO2 ZrO2 SnO2 TiO2 KNaO K2O Na2O CaO MgO ZnO BaO PbO Li2O SrO
Pink Nickel 6 0.14 1.24 0.12 0.03 0.09 0.01 0.01 0.33 0.45 0.09
IE81 6 0.14 1.24 0.12 0.03 0.09 0.01 0.01 0.33 0.45 0.09
B 242C 6 0.14 1.24 0.12 0.03 0.09 0.01 0.01 0.33 0.45 0.09

No reviews yet.

Hazards

09/2016 Note: This is a new feature. If a recipe material is not listed, that material's data has not yet been added. Some materials only have GHS ratings, while others only have HMIS ratings. Warnings differ between systems and countries. Glazy does not take any responsibility for accuracy of linked SDS information. Contact your ceramics supplier for safety information for your specific materials.
Globally Harmonized System (GHS) Hazardous Materials Identification System (HMIS) SDS Link
Material Pictograms Signal Word Hazard Statements Health Flammability Hazard Protection
Barium Carbonate Harmful WARNING Harmful if swallowed. 2 0 1 *
Silica HarmfulHealth Hazard DANGER From 200-Mesh SDS:
May cause cancer by inhalation.
Causes damage to lungs through prolonged or repeated exposure by inhalation.
* 0 0 E
Zinc Oxide 0 0 0 *
Lithium Carbonate Harmful WARNING Harmful if swallowed.
Causes serious eye irritation.
Harmful to aquatic life.
Bentonite Harmful WARNING Causes eye irritation
Causes skin irritation
May cause respiratory irritation
Nickel Oxide HarmfulHealth Hazard DANGER May cause an allergic skin reaction
May cause cancer by inhalation
Causes damage to organs through prolonged or repeated exposure