Category: Glaze > Crystalline
Created 2015-07-23 09:23:27 by Glazy Admin
Categories: Glaze > Crystalline
Firing Temperature: Δ6
Surface Type: Matte - Semi

Source/Alternate names: Clay Times Sept/Oct 2003

Source/Alternate names: similar oxides to Icing Pink

Firing Notes: cool maximum rate to 800C hold 1 hour

Notes: Alisa Clausen: A semi mat glaze that is has a smooth surface. Where thickest, it is slightly streaky and aqua, where thinnest, it is an
olive green.

Material Amount Batch Subtotal
Silica 41.48
Nepheline Syenite (Theoretical) 23.61
Whiting 12.39
Lithium Carbonate 11.26
Gerstley Borate 6.46
Magnesium carbonate 2.82
Barium Carbonate 1.98
Total Base:100
Rutile 3.55
Tin Oxide 3.05
Copper Carbonate 2.5
Total: 109.1

Percentage Analysis

Ingredient Amount SiO2 Al2O3 B2O3 MgO CaO BaO Li2O K2O Na2O KNaO P2O5 Fe2O3 TiO2 CuO SnO2 LOI
Silica41.4841.48
Nepheline Syenite (Theoretical)23.6114.335.50.020.171.092.313.40.020.17
Whiting12.396.955.44
Lithium Carbonate11.264.596.67
Gerstley Borate6.460.960.061.730.231.250.030.260.290.010.030.011.91
Magnesium carbonate2.821.351.47
Barium Carbonate1.981.540.44
Rutile3.550.353.2
Tin Oxide3.053.05
Copper Carbonate2.51.610.89
Total109.156.775.571.731.68.371.544.591.112.573.680.010.43.21.613.0516.99
100% no LOI 61.636.041.881.739.091.674.981.212.7940.010.433.481.753.31

Unity Molecular Formula (UMF)

FLUXES

RO/R2O

0.1 Na2O
0.03 K2O
0.38 Li2O
0.02 BaO
0.37 CaO
0.1 MgO
STABILIZERS

R2O3

0.13 Al2O3
0.06 B2O3
GLASS-FORMERS

RO2

2.33 SiO2
0.05 SnO2
0.1 TiO2
OTHER

 

0.01 Fe2O3
0.05 CuO
SILICA:ALUMINA

SiO2:Al2O3

17.31

FLUX RATIO

R2O:RO

0.51 : 0.49

SiO2:Al2O3 Chart

Closest 100 neighbors in Glaze > Crystalline.

Click and drag to zoom
Stull Chart
SiO2:Al2O3 Ratio
SiO2:Al2O3 Ratio 17.31

Similar Base Recipes

No recipes with similar base ingredients and amounts were found.

Similar RO/R2O Unity Formulas

R2O3 - STABILIZERS RO2 - GLASS FORMERS RO/R2O - FLUXES
Recipe Name ΔTemp Al2O3 B2O3 SiO2 ZrO2 SnO2 TiO2 KNaO K2O Na2O CaO MgO ZnO BaO PbO Li2O SrO
Crystalline Aqua Icing 6 0.13 0.06 2.33 0.05 0.1 0.13 0.03 0.1 0.37 0.1 0.02 0.38
Icing Pink 6 0.13 0.06 2.33 0.05 0.1 0.13 0.03 0.1 0.37 0.1 0.03 0.38

No reviews yet.

Hazards

09/2016 Note: This is a new feature. If a recipe material is not listed, that material's data has not yet been added. Some materials only have GHS ratings, while others only have HMIS ratings. Warnings differ between systems and countries. Glazy does not take any responsibility for accuracy of linked SDS information. Contact your ceramics supplier for safety information for your specific materials.
Globally Harmonized System (GHS) Hazardous Materials Identification System (HMIS) SDS Link
Material Pictograms Signal Word Hazard Statements Health Flammability Hazard Protection
Silica HarmfulHealth Hazard DANGER From 200-Mesh SDS:
May cause cancer by inhalation.
Causes damage to lungs through prolonged or repeated exposure by inhalation.
* 0 0 E
Whiting Harmful WARNING Causes eye irritation
Lithium Carbonate Harmful WARNING Harmful if swallowed.
Causes serious eye irritation.
Harmful to aquatic life.
Gerstley Borate
Magnesium carbonate WARNING Causes mild skin irritation
Causes eye irritation
Barium Carbonate Harmful WARNING Harmful if swallowed. 2 0 1 *
Rutile 1 0 0
Tin Oxide Harmful WARNING Harmful if swallowed.
Copper Carbonate Harmful WARNING Harmful if swallowed.
Causes skin irritation.
Causes serious eye irritation.