Category: Glaze > Clear
Created 2015-07-23 09:23:27 by Glazy Admin
Categories: Glaze > Clear
Firing Temperature: Δ6
Surface Type: Glossy

Notes: Alisa Clausen: A very fluid, gloss glaze with colours throughout varying from greenish brown to opal blues and whites. A lot of
movement in the glaze and one big pinhole where thickest under lip. Streaking on inside of bowl led to a pool of aqua gloss in middle
of bowl. Bulging edge of glaze on foot, almost a drip. Goes more opal white where thickest.

Material Amount Batch Subtotal
Frit 3134 20
Dolomite 20
Spodumene (Theoretical) 20
Ball Clay (Theoretical) 20
Silica 20
Tin Oxide 5
Copper Carbonate 2
Cobalt Carbonate 0.5
Total: 107.5

Percentage Analysis

Ingredient Amount SiO2 Al2O3 B2O3 MgO CaO Li2O K2O Na2O KNaO Fe2O3 TiO2 CoO CuO SnO2 LOI
Frit 3134209.34.624.032.062.06
Dolomite204.386.19.52
Spodumene (Theoretical)2012.925.481.6
Ball Clay (Theoretical)2011.8150.060.060.180.080.260.20.22.4
Silica2020
Tin Oxide55
Copper Carbonate21.290.71
Cobalt Carbonate0.50.320.19
Total107.554.0310.494.624.4410.181.60.182.132.310.20.20.321.29512.82
100% no LOI 57.0711.084.884.6910.751.690.192.252.440.220.210.331.365.28

Unity Molecular Formula (UMF)

FLUXES

RO/R2O

0.09 Na2O
0.01 K2O
0.14 Li2O
0.48 CaO
0.29 MgO
STABILIZERS

R2O3

0.27 Al2O3
0.17 B2O3
GLASS-FORMERS

RO2

2.36 SiO2
0.09 SnO2
0.01 TiO2
OTHER

 

0.01 CoO
0.04 CuO
SILICA:ALUMINA

SiO2:Al2O3

8.74

FLUX RATIO

R2O:RO

0.24 : 0.76

SiO2:Al2O3 Chart

Closest 100 neighbors in Glaze > Clear.

Click and drag to zoom
Stull Chart
SiO2:Al2O3 Ratio
SiO2:Al2O3 Ratio 8.74

Similar Base Recipes

No recipes with similar base ingredients and amounts were found.

Similar RO/R2O Unity Formulas

No recipes with similar RO/R2O Unity Formulas were found.

No reviews yet.

Hazards

09/2016 Note: This is a new feature. If a recipe material is not listed, that material's data has not yet been added. Some materials only have GHS ratings, while others only have HMIS ratings. Warnings differ between systems and countries. Glazy does not take any responsibility for accuracy of linked SDS information. Contact your ceramics supplier for safety information for your specific materials.
Globally Harmonized System (GHS) Hazardous Materials Identification System (HMIS) SDS Link
Material Pictograms Signal Word Hazard Statements Health Flammability Hazard Protection
Dolomite Health Hazard DANGER May cause cancer (Inhalation) 1 0 0 E
Spodumene (Theoretical) Health Hazard DANGER May cause cancer by inhalation.
Causes damage to organs through prolonged or repeated exposure.
Silica HarmfulHealth Hazard DANGER From 200-Mesh SDS:
May cause cancer by inhalation.
Causes damage to lungs through prolonged or repeated exposure by inhalation.
* 0 0 E
Tin Oxide Harmful WARNING Harmful if swallowed.
Copper Carbonate Harmful WARNING Harmful if swallowed.
Causes skin irritation.
Causes serious eye irritation.
Cobalt Carbonate Health HazardEnvironmental Hazard DANGER May cause cancer
Suspected of causing genetic effects
May damage fertility or the unborn child
May cause allergy or breathing difficulties if inhaled
May cause a allergic skin reaction
Very toxic to aquatic life
Very toxic to aquatic life with long lasting effects
2 0 0 *