Significant Flaw: crazing,potentially toxic

Notes: Alisa Clausen: a glossy medium to dark green, bright in colour. Shows signs of possible running where thickest. Crazed on my clay
body.

Material Amount Batch Subtotal
Silica 31.5
Nepheline Syenite (Theoretical) 24.7
Barium Carbonate 21.5
Strontium Carbonate 12.4
Kaolin (Theoretical) 7.1
Copper Carbonate 3
Whiting 2.8
Total: 103

Percentage Analysis

Ingredient Amount SiO2 Al2O3 MgO CaO SrO BaO K2O Na2O KNaO Fe2O3 CuO LOI
Silica31.531.5
Nepheline Syenite (Theoretical)24.714.995.750.020.171.142.423.560.020.17
Barium Carbonate21.516.74.8
Strontium Carbonate12.48.73.7
Kaolin (Theoretical)7.13.362.850.89
Copper Carbonate31.931.07
Whiting2.81.571.23
Total10349.858.610.021.748.716.71.142.423.560.021.9311.86
100% no LOI 54.699.450.031.919.5518.321.252.663.90.032.12

Unity Molecular Formula (UMF)

FLUXES

RO/R2O

0.14 Na2O
0.04 K2O
0.3 SrO
0.39 BaO
0.11 CaO
STABILIZERS

R2O3

0.31 Al2O3
GLASS-FORMERS

RO2

3.01 SiO2
OTHER

 

0.09 CuO
SILICA:ALUMINA

SiO2:Al2O3

9.83

FLUX RATIO

R2O:RO

0.19 : 0.81

SiO2:Al2O3 Chart

Closest 100 neighbors in Glaze > Green.

Click and drag to zoom
Stull Chart
SiO2:Al2O3 Ratio
SiO2:Al2O3 Ratio 9.83

Similar Base Recipes

No recipes with similar base ingredients and amounts were found.

Similar RO/R2O Unity Formulas

R2O3 - STABILIZERS RO2 - GLASS FORMERS RO/R2O - FLUXES
Recipe Name ΔTemp Al2O3 B2O3 SiO2 ZrO2 SnO2 TiO2 KNaO K2O Na2O CaO MgO ZnO BaO PbO Li2O SrO
Behrens Barium Base Green 6 0.31 3.01 0.18 0.04 0.14 0.11 0.39 0.3
Gloss 6 0.31 3 0.18 0.04 0.14 0.11 0.39 0.31
Behrens Barium Base 6 0.31 3.01 0.18 0.04 0.14 0.11 0.39 0.3
Behrens Barium Base Brown 6 0.31 3.01 0.18 0.04 0.14 0.11 0.39 0.3

No reviews yet.

Hazards

09/2016 Note: This is a new feature. If a recipe material is not listed, that material's data has not yet been added. Some materials only have GHS ratings, while others only have HMIS ratings. Warnings differ between systems and countries. Glazy does not take any responsibility for accuracy of linked SDS information. Contact your ceramics supplier for safety information for your specific materials.
Globally Harmonized System (GHS) Hazardous Materials Identification System (HMIS) SDS Link
Material Pictograms Signal Word Hazard Statements Health Flammability Hazard Protection
Silica HarmfulHealth Hazard DANGER From 200-Mesh SDS:
May cause cancer by inhalation.
Causes damage to lungs through prolonged or repeated exposure by inhalation.
* 0 0 E
Barium Carbonate Harmful WARNING Harmful if swallowed. 2 0 1 *
Strontium Carbonate Harmful WARNING Product dust may be irritating to eyes,skin and respiratory system.  1 0 0 E
Kaolin (Theoretical) HarmfulHealth Hazard DANGER SDS for EPK KAOLIN: EPK Kaolin is a naturally occurring mineral, which may contain amounts of crystalline silica
typically 0.1-1.0%, may cause damage to respiratory system through prolonged or repeated
exposure.
Copper Carbonate Harmful WARNING Harmful if swallowed.
Causes skin irritation.
Causes serious eye irritation.
Whiting Harmful WARNING Causes eye irritation