Category: Glaze > Red > Pink
Created 2015-07-23 09:23:27 by Glazy Admin
Categories: Glaze > Red > Pink
Firing Temperature: Δ6
Atmospheres: Oxidation
Surface Type: Matte - Semi

Source/Alternate names: Paul Lewing

Source/Alternate names: similar oxides to Crystalline Aqua Icing

Notes: Alisa Clausen: used Frit 623 for G.B. Smooth, well melted semi matte glaze, a ballerina tutu pink. It showed a white glaze where
very thick and a pink glaze where it broke thinner over the texture on test tile.

Material Amount Batch Subtotal
Silica 41.5
Nepheline Syenite (Theoretical) 23.6
Whiting 12.4
Lithium Carbonate 11.2
Gerstley Borate 6.5
Rutile 3.5
Tin Oxide 3
Magnesium carbonate 2.8
Barium Carbonate 2
Total: 106.5

Percentage Analysis

Ingredient Amount SiO2 Al2O3 B2O3 MgO CaO BaO Li2O K2O Na2O KNaO P2O5 Fe2O3 TiO2 SnO2 LOI
Silica41.541.5
Nepheline Syenite (Theoretical)23.614.335.50.020.171.092.313.40.020.17
Whiting12.46.965.44
Lithium Carbonate11.24.566.64
Gerstley Borate6.50.960.071.740.231.260.030.260.290.010.030.011.92
Rutile3.50.353.15
Tin Oxide33
Magnesium carbonate2.81.341.46
Barium Carbonate21.550.45
Total106.556.795.561.741.598.381.554.561.112.573.680.010.43.16316.08
100% no LOI 62.86.151.931.769.271.725.051.232.854.070.010.443.493.32

Unity Molecular Formula (UMF)

FLUXES

RO/R2O

0.1 Na2O
0.03 K2O
0.38 Li2O
0.03 BaO
0.37 CaO
0.1 MgO
STABILIZERS

R2O3

0.13 Al2O3
0.06 B2O3
GLASS-FORMERS

RO2

2.33 SiO2
0.05 SnO2
0.1 TiO2
OTHER

 

0.01 Fe2O3
SILICA:ALUMINA

SiO2:Al2O3

17.32

FLUX RATIO

R2O:RO

0.51 : 0.49

SiO2:Al2O3 Chart

Closest 28 neighbors in Glaze > Red > Pink.

Click and drag to zoom
Stull Chart
SiO2:Al2O3 Ratio
SiO2:Al2O3 Ratio 17.32

Similar Base Recipes

No recipes with similar base ingredients and amounts were found.

Similar RO/R2O Unity Formulas

R2O3 - STABILIZERS RO2 - GLASS FORMERS RO/R2O - FLUXES
Recipe Name ΔTemp Al2O3 B2O3 SiO2 ZrO2 SnO2 TiO2 KNaO K2O Na2O CaO MgO ZnO BaO PbO Li2O SrO
Icing Pink 6 0.13 0.06 2.33 0.05 0.1 0.13 0.03 0.1 0.37 0.1 0.03 0.38
Crystalline Aqua Icing 6 0.13 0.06 2.33 0.05 0.1 0.13 0.03 0.1 0.37 0.1 0.02 0.38

No reviews yet.

Hazards

09/2016 Note: This is a new feature. If a recipe material is not listed, that material's data has not yet been added. Some materials only have GHS ratings, while others only have HMIS ratings. Warnings differ between systems and countries. Glazy does not take any responsibility for accuracy of linked SDS information. Contact your ceramics supplier for safety information for your specific materials.
Globally Harmonized System (GHS) Hazardous Materials Identification System (HMIS) SDS Link
Material Pictograms Signal Word Hazard Statements Health Flammability Hazard Protection
Silica HarmfulHealth Hazard DANGER From 200-Mesh SDS:
May cause cancer by inhalation.
Causes damage to lungs through prolonged or repeated exposure by inhalation.
* 0 0 E
Whiting Harmful WARNING Causes eye irritation
Lithium Carbonate Harmful WARNING Harmful if swallowed.
Causes serious eye irritation.
Harmful to aquatic life.
Gerstley Borate
Rutile 1 0 0
Tin Oxide Harmful WARNING Harmful if swallowed.
Magnesium carbonate WARNING Causes mild skin irritation
Causes eye irritation
Barium Carbonate Harmful WARNING Harmful if swallowed. 2 0 1 *