Category: Glaze > Clear
Created 2015-10-14 00:04:17 by Tara Hagen
Categories: Glaze > Clear
Firing Temperature: Δ9-10
Atmospheres: Oxidation, Reduction
Surface Type: Glossy
Transparency: Translucent

Via Tara Hagen's Glazeitorium http://glazeitorium.blogspot.com/

Material Amount Batch Subtotal
K-200 Feldspar 87
Whiting 10
Total Base:97
Bentonite 3
Rutile 3
Red iron oxide 2
Total: 105

Percentage Analysis

Ingredient Amount SiO2 Al2O3 MgO CaO K2O Na2O KNaO Fe2O3 TiO2 LOI
K-200 Feldspar8759.2215.540.168.822.9311.750.070.27
Whiting105.614.39
Bentonite31.780.60.060.030.030.090.120.110.3
Rutile30.32.7
Red iron oxide21.90.1
Total1056116.140.065.88.853.0211.872.372.75.06
100% no LOI 61.0316.150.065.88.863.0211.882.372.7

Unity Molecular Formula (UMF)

FLUXES

RO/R2O

0.2 Na2O
0.38 K2O
0.42 CaO
0.01 MgO
STABILIZERS

R2O3

0.64 Al2O3
GLASS-FORMERS

RO2

4.1 SiO2
0.14 TiO2
OTHER

 

0.06 Fe2O3
SILICA:ALUMINA

SiO2:Al2O3

6.41

FLUX RATIO

R2O:RO

0.58 : 0.42

SiO2:Al2O3 Chart

Closest 100 neighbors in Glaze > Clear.

Click and drag to zoom
Stull Chart
SiO2:Al2O3 Ratio
SiO2:Al2O3 Ratio 6.41

Similar Base Recipes

No recipes with similar base ingredients and amounts were found.

Similar RO/R2O Unity Formulas

No recipes with similar RO/R2O Unity Formulas were found.

No reviews yet.

Hazards

09/2016 Note: This is a new feature. If a recipe material is not listed, that material's data has not yet been added. Some materials only have GHS ratings, while others only have HMIS ratings. Warnings differ between systems and countries. Glazy does not take any responsibility for accuracy of linked SDS information. Contact your ceramics supplier for safety information for your specific materials.
Globally Harmonized System (GHS) Hazardous Materials Identification System (HMIS) SDS Link
Material Pictograms Signal Word Hazard Statements Health Flammability Hazard Protection
Whiting Harmful WARNING Causes eye irritation
Bentonite Harmful WARNING Causes eye irritation
Causes skin irritation
May cause respiratory irritation
Rutile 1 0 0
Red iron oxide Health Hazard WARNING May cause damage to lung through prolonged or repeated exposure by inhalation