Category: Glaze > Red > Stain
Created 2015-10-19 02:51:38 by Terry Rorison
Categories: Glaze > Red > Stain
Firing Temperature: Δ6
Atmospheres: Oxidation
Surface Type: Glossy
Transparency: Transparent

Western Pennsylvania Potters Community

http://wpapotters.blogspot.com/2012/04/links-to-cone-6-oxidation-glaze-tests.html

http://www.wpapotters.blogspot.com/2010/11/cone-6-oxidation-results-group-3.html

With natural cooling in an electric kiln

Used Red Stain Standard Ceramic #487 8%

Material Amount Batch Subtotal
Frit 3134 27
Custer Feldspar 22.3
Silica 22.3
Whiting 11.8
EPK 9.9
Dolomite 3.6
Total Base:96.9
Mason stain 8
Bentonite 3.1
Total: 108

Percentage Analysis

Ingredient Amount SiO2 Al2O3 B2O3 MgO CaO K2O Na2O KNaO P2O5 Fe2O3 TiO2 LOI
Frit 31342712.566.235.432.772.77
Custer Feldspar22.315.283.790.072.230.672.90.020.07
Silica22.322.3
Whiting11.86.625.18
EPK9.94.533.70.010.020.030.010.040.030.080.041.47
Dolomite3.60.791.11.71
Mason stain8
Bentonite3.11.840.620.060.030.030.090.120.110.31
Total10856.58.116.230.8613.272.33.545.840.030.210.048.74
100% no LOI 62.038.916.840.9514.572.523.896.410.030.230.04

Unity Molecular Formula (UMF)

FLUXES

RO/R2O

0.17 Na2O
0.07 K2O
0.7 CaO
0.06 MgO
STABILIZERS

R2O3

0.24 Al2O3
0.26 B2O3
GLASS-FORMERS

RO2

2.77 SiO2
SILICA:ALUMINA

SiO2:Al2O3

11.80

FLUX RATIO

R2O:RO

0.24 : 0.76

SiO2:Al2O3 Chart

Closest 7 neighbors in Glaze > Red > Stain.

Click and drag to zoom
Stull Chart
SiO2:Al2O3 Ratio
SiO2:Al2O3 Ratio 11.8

Similar RO/R2O Unity Formulas

R2O3 - STABILIZERS RO2 - GLASS FORMERS RO/R2O - FLUXES
Recipe Name ΔTemp Al2O3 B2O3 SiO2 ZrO2 SnO2 TiO2 KNaO K2O Na2O CaO MgO ZnO BaO PbO Li2O SrO
GA 20 Cone 6 Lewings SC40E Red 6 0.24 0.26 2.77 0.24 0.07 0.17 0.7 0.06
GA 20 Cone 6 Lewings SC40E Blue Gray 6 0.24 0.26 2.77 0.24 0.07 0.17 0.7 0.06

No reviews yet.

Hazards

09/2016 Note: This is a new feature. If a recipe material is not listed, that material's data has not yet been added. Some materials only have GHS ratings, while others only have HMIS ratings. Warnings differ between systems and countries. Glazy does not take any responsibility for accuracy of linked SDS information. Contact your ceramics supplier for safety information for your specific materials.
Globally Harmonized System (GHS) Hazardous Materials Identification System (HMIS) SDS Link
Material Pictograms Signal Word Hazard Statements Health Flammability Hazard Protection
Custer Feldspar HarmfulHealth Hazard WARNING May cause damage to lungs through prolonged or repeated inhalation.
Suspected of causing cancer through
prolonged or repeated inhalation.
May cause allergy or asthma symptoms or breathing difficulties if inhaled.
May cause skin or eye irritation.
Silica HarmfulHealth Hazard DANGER From 200-Mesh SDS:
May cause cancer by inhalation.
Causes damage to lungs through prolonged or repeated exposure by inhalation.
* 0 0 E
Whiting Harmful WARNING Causes eye irritation
EPK HarmfulHealth Hazard DANGER EPK Kaolin is a naturally occurring mineral, which may contain amounts of crystalline silica
typically 0.1-1.0%, may cause damage to respiratory system through prolonged or repeated
exposure.
1 0 0 E
Dolomite Health Hazard DANGER May cause cancer (Inhalation) 1 0 0 E
Bentonite Harmful WARNING Causes eye irritation
Causes skin irritation
May cause respiratory irritation