Category: Glaze
Created 2015-10-19 03:24:09 by Terry Rorison
Categories: Glaze
Firing Temperature: Δ6
Atmospheres: Oxidation
Surface Type: Satin
Transparency: Translucent
Material Amount Batch Subtotal
Minspar 200 41
Silica 19
Zircopax 12
Whiting 7
Dolomite 5
Zinc Oxide 2
Tennessee ball clay 1
Total Base:87
Copper Carbonate 2.5
Total: 89.5

Percentage Analysis

Ingredient Amount SiO2 Al2O3 MgO CaO ZnO K2O Na2O KNaO Fe2O3 TiO2 CuO ZrO2 LOI
Minspar 2004128.257.620.621.692.684.370.020.12
Silica1919
Zircopax123.938.07
Whiting73.933.07
Dolomite51.11.522.38
Zinc Oxide22
Tennessee ball clay10.540.30.010.010.020.11
Copper Carbonate2.51.610.89
Total89.551.737.921.16.0721.692.684.370.040.021.618.076.58
100%57.88.851.236.792.231.892.994.890.040.021.89.017.35
100% no LOI 62.389.551.337.322.412.043.235.270.040.021.949.73

Unity Molecular Formula (UMF)

FLUXES

RO/R2O

0.2 Na2O
0.08 K2O
0.11 ZnO
0.49 CaO
0.12 MgO
STABILIZERS

R2O3

0.35 Al2O3
GLASS-FORMERS

RO2

3.89 SiO2
0.3 ZrO2
OTHER

 

0.09 CuO
SILICA:ALUMINA

SiO2:Al2O3

11.08

FLUX RATIO

R2O:RO

0.28 : 0.72

SiO2:Al2O3 Chart

Closest 100 neighbors in Glaze.

Click and drag to zoom
Stull Chart
SiO2:Al2O3 Ratio
SiO2:Al2O3 Ratio 11.08

Similar Base Recipes

No recipes with similar base ingredients and amounts were found.

Similar RO/R2O Unity Formulas

No recipes with similar RO/R2O Unity Formulas were found.

No reviews yet.

Hazards

09/2016 Note: This is a new feature. If a recipe material is not listed, that material's data has not yet been added. Some materials only have GHS ratings, while others only have HMIS ratings. Warnings differ between systems and countries. Glazy does not take any responsibility for accuracy of linked SDS information. Contact your ceramics supplier for safety information for your specific materials.
Globally Harmonized System (GHS) Hazardous Materials Identification System (HMIS) SDS Link
Material Pictograms Signal Word Hazard Statements Health Flammability Hazard Protection
Minspar 200 Health Hazard WARNING May cause damage to lung through prolonged or repeated inhalation 2 0 0 E
Silica HarmfulHealth Hazard DANGER From 200-Mesh SDS:
May cause cancer by inhalation.
Causes damage to lungs through prolonged or repeated exposure by inhalation.
* 0 0 E
Zircopax
Whiting Harmful WARNING Causes eye irritation
Dolomite Health Hazard DANGER May cause cancer (Inhalation) 1 0 0 E
Zinc Oxide 0 0 0 *
Tennessee ball clay Health Hazard WARNING May cause damage to lung through prolonged or repeated inhalation 2 0 0 E
Copper Carbonate Harmful WARNING Harmful if swallowed.
Causes skin irritation.
Causes serious eye irritation.