Category: Glaze > Green > Copper
Created 2015-10-20 02:10:35 by Terry Rorison
Categories: Glaze > Green > Copper
Firing Temperature: Δ6
Atmospheres: Oxidation
Surface Type: Glossy
Transparency: Translucent
Material Amount Batch Subtotal
Minspar 200 47
Whiting 18
Kentucky OM #4 Ball Clay 14
Gillespie Borate 9
Silica 6
Total Base:94
Copper Carbonate 5
Red iron oxide 1
Total: 100

Percentage Analysis

Ingredient Amount SiO2 Al2O3 B2O3 MgO CaO SrO K2O Na2O KNaO Fe2O3 TiO2 CuO LOI
Minspar 2004732.398.730.711.943.075.010.030.14
Whiting1810.17.9
Kentucky OM #4 Ball Clay147.733.910.060.040.140.040.180.150.171.76
Gillespie Borate91.060.152.20.352.070.040.340.342.78
Silica66
Copper Carbonate53.221.78
Red iron oxide10.950.05
Total10047.1812.792.20.4112.920.042.083.455.531.130.173.2214.42
100% no LOI 55.1214.952.580.4815.090.052.434.036.461.320.23.76

Unity Molecular Formula (UMF)

FLUXES

RO/R2O

0.17 Na2O
0.07 K2O
0.72 CaO
0.03 MgO
STABILIZERS

R2O3

0.39 Al2O3
0.1 B2O3
GLASS-FORMERS

RO2

2.46 SiO2
0.01 TiO2
OTHER

 

0.02 Fe2O3
0.13 CuO
SILICA:ALUMINA

SiO2:Al2O3

6.26

FLUX RATIO

R2O:RO

0.24 : 0.76

SiO2:Al2O3 Chart

Closest 100 neighbors in Glaze > Green > Copper.

Click and drag to zoom
Stull Chart
SiO2:Al2O3 Ratio
SiO2:Al2O3 Ratio 6.26

Similar Base Recipes

No recipes with similar base ingredients and amounts were found.

Similar RO/R2O Unity Formulas

R2O3 - STABILIZERS RO2 - GLASS FORMERS RO/R2O - FLUXES
Recipe Name ΔTemp Al2O3 B2O3 SiO2 ZrO2 SnO2 TiO2 KNaO K2O Na2O CaO MgO ZnO BaO PbO Li2O SrO
Transparent Dark Green Glossy Cone 6 6 0.39 0.1 2.46 0.01 0.24 0.07 0.17 0.72 0.03
Matte Satin VC 5-6 0.39 0.14 2.44 0.23 0.04 0.19 0.77

No reviews yet.

Hazards

09/2016 Note: This is a new feature. If a recipe material is not listed, that material's data has not yet been added. Some materials only have GHS ratings, while others only have HMIS ratings. Warnings differ between systems and countries. Glazy does not take any responsibility for accuracy of linked SDS information. Contact your ceramics supplier for safety information for your specific materials.
Globally Harmonized System (GHS) Hazardous Materials Identification System (HMIS) SDS Link
Material Pictograms Signal Word Hazard Statements Health Flammability Hazard Protection
Minspar 200 Health Hazard WARNING May cause damage to lung through prolonged or repeated inhalation 2 0 0 E
Whiting Harmful WARNING Causes eye irritation
Kentucky OM #4 Ball Clay Health Hazard WARNING May cause damage to lung through prolonged or repeated inhalation 2 0 0 E
Silica HarmfulHealth Hazard DANGER From 200-Mesh SDS:
May cause cancer by inhalation.
Causes damage to lungs through prolonged or repeated exposure by inhalation.
* 0 0 E
Copper Carbonate Harmful WARNING Harmful if swallowed.
Causes skin irritation.
Causes serious eye irritation.
Red iron oxide Health Hazard WARNING May cause damage to lung through prolonged or repeated exposure by inhalation