Category: Glaze > Blue
Created 2015-10-20 02:12:47 by Terry Rorison
Categories: Glaze > Blue
Firing Temperature: Δ6
Atmospheres: Oxidation
Surface Type: Matte
Transparency: Opaque
Material Amount Batch Subtotal
Minspar 200 50
Whiting 18
EPK 15
Zinc Oxide 8
Silica 4
Total Base:95
Bentonite 2
Rutile 2
Cobalt Carbonate 1
Total: 100

Percentage Analysis

Ingredient Amount SiO2 Al2O3 MgO CaO ZnO K2O Na2O KNaO P2O5 Fe2O3 TiO2 CoO LOI
Minspar 2005034.459.290.752.063.265.320.030.15
Whiting1810.17.9
EPK156.865.60.020.030.050.010.060.040.110.062.22
Zinc Oxide88
Silica44
Bentonite21.190.40.040.020.020.060.080.070.2
Rutile20.21.8
Cobalt Carbonate10.630.37
Total10046.515.30.0610.982.133.345.470.040.411.860.6310.85
100% no LOI 52.1517.160.0612.228.972.393.746.130.040.462.080.71

Unity Molecular Formula (UMF)

FLUXES

RO/R2O

0.15 Na2O
0.06 K2O
0.27 ZnO
0.52 CaO
STABILIZERS

R2O3

0.4 Al2O3
GLASS-FORMERS

RO2

2.09 SiO2
0.06 TiO2
OTHER

 

0.01 Fe2O3
0.02 CoO
SILICA:ALUMINA

SiO2:Al2O3

5.16

FLUX RATIO

R2O:RO

0.21 : 0.79

SiO2:Al2O3 Chart

Closest 100 neighbors in Glaze > Blue.

Click and drag to zoom
Stull Chart
SiO2:Al2O3 Ratio
SiO2:Al2O3 Ratio 5.16

Similar Base Recipes

No recipes with similar base ingredients and amounts were found.

Similar RO/R2O Unity Formulas

No recipes with similar RO/R2O Unity Formulas were found.

No reviews yet.

Hazards

09/2016 Note: This is a new feature. If a recipe material is not listed, that material's data has not yet been added. Some materials only have GHS ratings, while others only have HMIS ratings. Warnings differ between systems and countries. Glazy does not take any responsibility for accuracy of linked SDS information. Contact your ceramics supplier for safety information for your specific materials.
Globally Harmonized System (GHS) Hazardous Materials Identification System (HMIS) SDS Link
Material Pictograms Signal Word Hazard Statements Health Flammability Hazard Protection
Minspar 200 Health Hazard WARNING May cause damage to lung through prolonged or repeated inhalation 2 0 0 E
Whiting Harmful WARNING Causes eye irritation
EPK HarmfulHealth Hazard DANGER EPK Kaolin is a naturally occurring mineral, which may contain amounts of crystalline silica
typically 0.1-1.0%, may cause damage to respiratory system through prolonged or repeated
exposure.
1 0 0 E
Zinc Oxide 0 0 0 *
Silica HarmfulHealth Hazard DANGER From 200-Mesh SDS:
May cause cancer by inhalation.
Causes damage to lungs through prolonged or repeated exposure by inhalation.
* 0 0 E
Bentonite Harmful WARNING Causes eye irritation
Causes skin irritation
May cause respiratory irritation
Rutile 1 0 0
Cobalt Carbonate Health HazardEnvironmental Hazard DANGER May cause cancer
Suspected of causing genetic effects
May damage fertility or the unborn child
May cause allergy or breathing difficulties if inhaled
May cause a allergic skin reaction
Very toxic to aquatic life
Very toxic to aquatic life with long lasting effects
2 0 0 *