Category: Glaze > Shino
Created 2016-01-25 09:12:50 by Daniel Spruyt
Categories: Glaze > Shino
Firing Temperature: Δ6-7
Atmospheres: Oxidation
Surface Type: Satin
Transparency: Opaque

Nutmeg Shino Cone 6 Sugar Maples (original name from authors: http://wpapotters.blogspot.be/2010/11/cone-6-oxidation-results-group-3.html )
A good example why recipes don't always travel well, although I was pleased with the result. With my materials (Belgium) I got a nice glaze with excellent breaking. I don't know where the term "Sugar Maples" applies and what kind of nutmeg authors had in mind...

Material Amount Batch Subtotal
Dolomite 23.3
Spodumene (Theoretical) 23.3
Ball Clay (Theoretical) 23.3
Silica 23.3
Frit 3134 6.8
Total Base:100
Tin Oxide 5
Yellow Ochre 3
Iron oxide 1
Total: 109

Percentage Analysis

Ingredient Amount SiO2 Al2O3 B2O3 MgO CaO Li2O K2O Na2O KNaO Fe2O3 TiO2 SnO2 LOI
Dolomite23.35.17.111.09
Spodumene (Theoretical)23.315.056.391.87
Ball Clay (Theoretical)23.313.765.830.070.070.210.090.30.240.232.8
Silica23.323.3
Frit 31346.83.161.571.370.70.7
Tin Oxide55
Yellow Ochre31.730.60.010.66
Iron oxide10.950.05
Total10957.0112.811.575.188.551.870.210.7911.850.23513.94
100% no LOI 59.9713.481.655.448.991.960.220.831.051.940.255.26

Unity Molecular Formula (UMF)

FLUXES

RO/R2O

0.04 Na2O
0.01 K2O
0.17 Li2O
0.43 CaO
0.36 MgO
STABILIZERS

R2O3

0.35 Al2O3
0.06 B2O3
GLASS-FORMERS

RO2

2.65 SiO2
0.09 SnO2
0.01 TiO2
OTHER

 

0.03 Fe2O3
SILICA:ALUMINA

SiO2:Al2O3

7.55

FLUX RATIO

R2O:RO

0.22 : 0.78

SiO2:Al2O3 Chart

Closest 100 neighbors in Glaze > Shino.

Click and drag to zoom
Stull Chart
SiO2:Al2O3 Ratio
SiO2:Al2O3 Ratio 7.55

Similar RO/R2O Unity Formulas

R2O3 - STABILIZERS RO2 - GLASS FORMERS RO/R2O - FLUXES
Recipe Name ΔTemp Al2O3 B2O3 SiO2 ZrO2 SnO2 TiO2 KNaO K2O Na2O CaO MgO ZnO BaO PbO Li2O SrO
WWW 486 6-7 0.35 0.06 2.65 0.09 0.01 0.05 0.01 0.04 0.43 0.36 0.17
Nutmeg Shino Cone 6 Sugar Maples 6 0.37 0.06 2.61 0.09 0.01 0.04 0.01 0.03 0.42 0.36 0.17
Nutmeg Shino Cone 6 Sugar Maples (Toms UK GB variation) 6-7 0.37 0.06 2.62 0.1 0.02 0.01 0.01 0.42 0.37 0.18
Nutmeg Richard Busch's 6 0.38 0.06 2.65 0.09 0.01 0.05 0.01 0.04 0.42 0.36 0.17
Chromed Nutmeg 5-6 0.38 0.06 2.65 0.09 0.01 0.05 0.01 0.04 0.42 0.36 0.17
Nutmeg (variation) 6 0.36 0.06 2.69 0.09 0.01 0.05 0.01 0.04 0.42 0.36 0.17

No reviews yet.

Hazards

09/2016 Note: This is a new feature. If a recipe material is not listed, that material's data has not yet been added. Some materials only have GHS ratings, while others only have HMIS ratings. Warnings differ between systems and countries. Glazy does not take any responsibility for accuracy of linked SDS information. Contact your ceramics supplier for safety information for your specific materials.
Globally Harmonized System (GHS) Hazardous Materials Identification System (HMIS) SDS Link
Material Pictograms Signal Word Hazard Statements Health Flammability Hazard Protection
Dolomite Health Hazard DANGER May cause cancer (Inhalation) 1 0 0 E
Spodumene (Theoretical) Health Hazard DANGER May cause cancer by inhalation.
Causes damage to organs through prolonged or repeated exposure.
Silica HarmfulHealth Hazard DANGER From 200-Mesh SDS:
May cause cancer by inhalation.
Causes damage to lungs through prolonged or repeated exposure by inhalation.
* 0 0 E
Tin Oxide Harmful WARNING Harmful if swallowed.
Yellow Ochre Health Hazard DANGER May cause cancer.
Iron oxide Health Hazard WARNING SDS for Red Iron Oxide: May cause damage to lung through prolonged or repeated exposure by inhalation