Category: Glaze > Clear
Created 2016-01-30 22:09:08 by Nate Willever
Categories: Glaze > Clear
Firing Temperature: Δ5½-6
Atmospheres: Oxidation
Surface Type: Glossy
Transparency: Transparent

Runny Clear, Cone 6

Material Amount Batch Subtotal
Nepheline Syenite (Theoretical) 22
Wollastonite (Theoretical) 22
Frit 3134 22
Silica 16.5
EPK 16.5
Talc (Theoretical) 1
Total: 100

Percentage Analysis

Ingredient Amount SiO2 Al2O3 B2O3 MgO CaO K2O Na2O KNaO P2O5 Fe2O3 TiO2 LOI
Nepheline Syenite (Theoretical)2213.355.130.020.151.012.163.170.020.15
Wollastonite (Theoretical)2211.3810.62
Frit 31342210.235.084.432.262.26
Silica16.516.5
EPK16.57.546.160.020.030.060.010.070.040.130.062.44
Talc (Theoretical)10.630.320.05
Total10059.6411.295.080.3615.231.074.435.50.040.150.062.65
100% no LOI 61.2611.65.220.3715.651.14.555.650.040.150.06

Unity Molecular Formula (UMF)

FLUXES

RO/R2O

0.2 Na2O
0.03 K2O
0.75 CaO
0.02 MgO
STABILIZERS

R2O3

0.3 Al2O3
0.2 B2O3
GLASS-FORMERS

RO2

2.73 SiO2
SILICA:ALUMINA

SiO2:Al2O3

8.96

FLUX RATIO

R2O:RO

0.23 : 0.77

SiO2:Al2O3 Chart

Closest 100 neighbors in Glaze > Clear.

Click and drag to zoom
Stull Chart
SiO2:Al2O3 Ratio
SiO2:Al2O3 Ratio 8.96

Similar Base Recipes

No recipes with similar base ingredients and amounts were found.

Similar RO/R2O Unity Formulas

R2O3 - STABILIZERS RO2 - GLASS FORMERS RO/R2O - FLUXES
Recipe Name ΔTemp Al2O3 B2O3 SiO2 ZrO2 SnO2 TiO2 KNaO K2O Na2O CaO MgO ZnO BaO PbO Li2O SrO
Willever Clear 5½-6 0.3 0.2 2.73 0.23 0.03 0.2 0.75 0.02
Transparent Gloss #3 6 0.33 0.22 2.68 0.24 0.14 0.1 0.71 0.05
Alexandra FitzGerald 2016-10-12 15:39:10
This is a super lovely clear. I'll upload my test tiles soon. Doesn't run but does move a little bit, making some nice variation in lines. Overall I'm very pleased with this clear!

Hazards

09/2016 Note: This is a new feature. If a recipe material is not listed, that material's data has not yet been added. Some materials only have GHS ratings, while others only have HMIS ratings. Warnings differ between systems and countries. Glazy does not take any responsibility for accuracy of linked SDS information. Contact your ceramics supplier for safety information for your specific materials.
Globally Harmonized System (GHS) Hazardous Materials Identification System (HMIS) SDS Link
Material Pictograms Signal Word Hazard Statements Health Flammability Hazard Protection
Wollastonite (Theoretical) Health Hazard DANGER Vansil W-30 Wollastonite SDS:
May cause cancer if inhaled.
Causes damage to organs through prolonged or repeated exposure if inhaled. (respiratory tract)
Silica HarmfulHealth Hazard DANGER From 200-Mesh SDS:
May cause cancer by inhalation.
Causes damage to lungs through prolonged or repeated exposure by inhalation.
* 0 0 E
EPK HarmfulHealth Hazard DANGER EPK Kaolin is a naturally occurring mineral, which may contain amounts of crystalline silica
typically 0.1-1.0%, may cause damage to respiratory system through prolonged or repeated
exposure.
1 0 0 E
Talc (Theoretical) Harmful WARNING Causes mild skin irritation
Harmful if inhaled
May cause respiratory irritation
1 0 0 E