Category: Glaze > Specialty > Metallic
Created 2016-03-22 20:14:51 by Steve Davis
Categories: Glaze > Specialty > Metallic
Firing Temperature: Δ5-9
Atmospheres: Oxidation

From Steve Davis

Website: http://kazegamas.com/
Golds / Cone 5-9 Oxidation: http://kazegamas.com/Golds-C5.htm

Material Amount Batch Subtotal
Redart 85
Frit 3124 15
Total Base:100
Manganese Dioxide 65
Copper Oxide 5
Cobalt Oxide 5
Total: 175

Percentage Analysis

Ingredient Amount SiO2 Al2O3 B2O3 MgO CaO K2O Na2O KNaO P2O5 Fe2O3 TiO2 MnO2 CoO CuO LOI
Redart8555.2113.181.350.223.530.323.850.195.990.934.08
Frit 3124158.31.482.072.110.10.941.04
Manganese Dioxide6556.498.52
Copper Oxide55
Cobalt Oxide54.670.33
Total17563.514.672.071.352.333.631.274.890.195.990.9356.494.67512.93
100% no LOI 39.189.051.270.831.442.240.783.020.123.70.5734.852.883.09

Unity Molecular Formula (UMF)

FLUXES

RO/R2O

0.15 Na2O
0.29 K2O
0.31 CaO
0.25 MgO
STABILIZERS

R2O3

1.07 Al2O3
0.22 B2O3
GLASS-FORMERS

RO2

7.88 SiO2
0.09 TiO2
OTHER

 

0.28 Fe2O3
4.85 MnO2
0.01 P2O5
0.46 CoO
0.47 CuO
SILICA:ALUMINA

SiO2:Al2O3

7.35

FLUX RATIO

R2O:RO

0.44 : 0.56

SiO2:Al2O3 Chart

Closest 43 neighbors in Glaze > Specialty > Metallic.

Click and drag to zoom
Stull Chart
SiO2:Al2O3 Ratio
SiO2:Al2O3 Ratio 7.35

Similar Base Recipes

No recipes with similar base ingredients and amounts were found.

Similar RO/R2O Unity Formulas

No recipes with similar RO/R2O Unity Formulas were found.

No reviews yet.

Hazards

09/2016 Note: This is a new feature. If a recipe material is not listed, that material's data has not yet been added. Some materials only have GHS ratings, while others only have HMIS ratings. Warnings differ between systems and countries. Glazy does not take any responsibility for accuracy of linked SDS information. Contact your ceramics supplier for safety information for your specific materials.
Globally Harmonized System (GHS) Hazardous Materials Identification System (HMIS) SDS Link
Material Pictograms Signal Word Hazard Statements Health Flammability Hazard Protection
Redart HarmfulHealth Hazard DANGER Causes skin irritation
Causes eye irritation
May cause cancer (Inhalation)
Manganese Dioxide Harmful WARNING Harmful if swallowed. Causes serious eye irritation. Harmful if inhaled. May cause respiratory
irritation.
Copper Oxide Harmful WARNING Harmful if swallowed 2 0 0 E
Cobalt Oxide HarmfulHealth Hazard WARNING Suspected of causing cancer
Harmful if swallowed
May cause allergy or breathing difficulties if inhaled
May cause an allergic skin reaction
2 0 0 *