Here's a couple that I have tried and added to my regulars (both come
from clayart folks). The Moonlight will run if applied to thick. If
you are looking for a shiny glaze try the Moonlight. Chris Fennimore
Native American Rights Fund Boulder, CO christine fennimore

Material Amount Batch Subtotal
Cornwall Stone 63.8
Gerstley Borate 14.3
Silica 7.6
Whiting 7.6
EPK 4.8
Zinc Oxide 1.9
Total Base:100
Rutile 3.2
Ilmenite 2.04
Total: 105.24

Percentage Analysis

Ingredient Amount SiO2 Al2O3 B2O3 MgO CaO ZnO K2O Na2O KNaO P2O5 FeO Fe2O3 TiO2 LOI
Cornwall Stone63.847.0710.420.091.162.742.14.840.120.1
Gerstley Borate14.32.120.143.830.52.770.060.570.630.010.060.014.22
Silica7.67.6
Whiting7.64.263.34
EPK4.82.191.790.010.020.020.010.040.020.71
Zinc Oxide1.91.9
Rutile3.20.322.88
Ilmenite2.040.971.07
Total105.2458.9812.353.830.68.21.92.822.685.50.030.970.534.088.27
100% no LOI 60.8212.743.950.618.461.962.912.765.670.0310.554.21

Unity Molecular Formula (UMF)

FLUXES

RO/R2O

0.17 Na2O
0.12 K2O
0.09 ZnO
0.57 CaO
0.06 MgO
STABILIZERS

R2O3

0.47 Al2O3
0.21 B2O3
GLASS-FORMERS

RO2

3.81 SiO2
0.2 TiO2
OTHER

 

0.01 Fe2O3
0.05 FeO
SILICA:ALUMINA

SiO2:Al2O3

8.10

FLUX RATIO

R2O:RO

0.28 : 0.72

SiO2:Al2O3 Chart

Closest 19 neighbors in Glaze > Blue > Rutile.

Click and drag to zoom
Stull Chart
SiO2:Al2O3 Ratio
SiO2:Al2O3 Ratio 8.1

Similar Base Recipes

Similar RO/R2O Unity Formulas

R2O3 - STABILIZERS RO2 - GLASS FORMERS RO/R2O - FLUXES
Recipe Name ΔTemp Al2O3 B2O3 SiO2 ZrO2 SnO2 TiO2 KNaO K2O Na2O CaO MgO ZnO BaO PbO Li2O SrO
Moonlight 10 0.47 0.21 3.81 0.2 0.29 0.12 0.17 0.57 0.06 0.09
Conrad G375 Moonlight Blue 10 0.47 0.21 3.81 0.2 0.29 0.12 0.17 0.57 0.06 0.09
kelso lokey 2017-09-07 02:12:14
i made this glaze at my university studio. it got renamed "every little girl's dream". i liked it in wood and soda fires

Hazards

09/2016 Note: This is a new feature. If a recipe material is not listed, that material's data has not yet been added. Some materials only have GHS ratings, while others only have HMIS ratings. Warnings differ between systems and countries. Glazy does not take any responsibility for accuracy of linked SDS information. Contact your ceramics supplier for safety information for your specific materials.
Globally Harmonized System (GHS) Hazardous Materials Identification System (HMIS) SDS Link
Material Pictograms Signal Word Hazard Statements Health Flammability Hazard Protection
Gerstley Borate
Silica HarmfulHealth Hazard DANGER From 200-Mesh SDS:
May cause cancer by inhalation.
Causes damage to lungs through prolonged or repeated exposure by inhalation.
* 0 0 E
Whiting Harmful WARNING Causes eye irritation
EPK HarmfulHealth Hazard DANGER EPK Kaolin is a naturally occurring mineral, which may contain amounts of crystalline silica
typically 0.1-1.0%, may cause damage to respiratory system through prolonged or repeated
exposure.
1 0 0 E
Zinc Oxide 0 0 0 *
Rutile 1 0 0
Ilmenite