Category: Glaze > Red > Stain
Created 2016-06-20 19:01:02 by Ginger Lukas
Categories: Glaze > Red > Stain
Firing Temperature: Δ04
Atmospheres: Oxidation
Surface Type: Matte - Semi
Transparency: Opaque

This one settles like a rock. I would recommend Darvan or Epsom salt or something like it or you'll be sieving for hours. Val Cushing Base.

Material Amount Batch Subtotal
Frit 3110 70.1
Silica 8.8
Gerstley Borate 7.6
Soda Ash 7.5
EPK 6
Total Base:100
Zircopax 14
Red stain 8
Total: 122

Percentage Analysis

Ingredient Amount SiO2 Al2O3 B2O3 MgO CaO K2O Na2O KNaO P2O5 Fe2O3 TiO2 ZrO2 LOI
Frit 311070.146.884.222.033.952.4210.613.02
Silica8.88.8
Gerstley Borate7.61.120.082.040.271.470.030.30.330.010.030.012.24
Soda Ash7.53.753.753.75
EPK62.742.240.010.010.020.020.020.050.020.89
Zircopax144.599.41
Red stain8
Total12264.146.544.060.275.442.4714.6517.120.020.080.039.416.88
100% no LOI 59.886.13.790.255.082.313.6815.980.020.070.038.79

Unity Molecular Formula (UMF)

FLUXES

RO/R2O

0.65 Na2O
0.07 K2O
0.26 CaO
0.02 MgO
STABILIZERS

R2O3

0.18 Al2O3
0.16 B2O3
GLASS-FORMERS

RO2

2.91 SiO2
0.21 ZrO2
SILICA:ALUMINA

SiO2:Al2O3

16.64

FLUX RATIO

R2O:RO

0.72 : 0.28

SiO2:Al2O3 Chart

Closest 7 neighbors in Glaze > Red > Stain.

Click and drag to zoom
Stull Chart
SiO2:Al2O3 Ratio
SiO2:Al2O3 Ratio 16.64

Similar Base Recipes

Δ05½ - 04

Similar RO/R2O Unity Formulas

No recipes with similar RO/R2O Unity Formulas were found.

No reviews yet.

Hazards

09/2016 Note: This is a new feature. If a recipe material is not listed, that material's data has not yet been added. Some materials only have GHS ratings, while others only have HMIS ratings. Warnings differ between systems and countries. Glazy does not take any responsibility for accuracy of linked SDS information. Contact your ceramics supplier for safety information for your specific materials.
Globally Harmonized System (GHS) Hazardous Materials Identification System (HMIS) SDS Link
Material Pictograms Signal Word Hazard Statements Health Flammability Hazard Protection
Silica HarmfulHealth Hazard DANGER From 200-Mesh SDS:
May cause cancer by inhalation.
Causes damage to lungs through prolonged or repeated exposure by inhalation.
* 0 0 E
Gerstley Borate
Soda Ash Harmful WARNING Causes skin irritation.
Causes serious eye irritation.
2 0 0 B
EPK HarmfulHealth Hazard DANGER EPK Kaolin is a naturally occurring mineral, which may contain amounts of crystalline silica
typically 0.1-1.0%, may cause damage to respiratory system through prolonged or repeated
exposure.
1 0 0 E
Zircopax