Material Amount Batch Subtotal
Minspar 200 43.4
Wollastonite (Theoretical) 20
Frit 3134 20
EPK 17
Total Base:100.4
Rutile 6
Total: 106.4

Percentage Analysis

Ingredient Amount SiO2 Al2O3 B2O3 MgO CaO K2O Na2O KNaO P2O5 Fe2O3 TiO2 LOI
Minspar 20043.429.98.060.651.792.834.620.030.13
Wollastonite (Theoretical)2010.349.66
Frit 3134209.34.624.032.062.06
EPK177.776.350.020.030.060.010.070.040.130.062.52
Rutile60.595.40.01
Total106.457.3214.424.620.0214.371.854.96.750.040.755.462.65
100% no LOI 55.2513.94.450.0213.851.784.726.50.040.725.27

Unity Molecular Formula (UMF)

FLUXES

RO/R2O

0.22 Na2O
0.06 K2O
0.72 CaO
STABILIZERS

R2O3

0.4 Al2O3
0.19 B2O3
GLASS-FORMERS

RO2

2.69 SiO2
0.19 TiO2
OTHER

 

0.01 Fe2O3
SILICA:ALUMINA

SiO2:Al2O3

6.75

FLUX RATIO

R2O:RO

0.28 : 0.72

SiO2:Al2O3 Chart

Closest 29 neighbors in Glaze > Yellow > Iron.

Click and drag to zoom
Stull Chart
SiO2:Al2O3 Ratio
SiO2:Al2O3 Ratio 6.75

Similar Base Recipes

Similar RO/R2O Unity Formulas

No recipes with similar RO/R2O Unity Formulas were found.

No reviews yet.

Hazards

09/2016 Note: This is a new feature. If a recipe material is not listed, that material's data has not yet been added. Some materials only have GHS ratings, while others only have HMIS ratings. Warnings differ between systems and countries. Glazy does not take any responsibility for accuracy of linked SDS information. Contact your ceramics supplier for safety information for your specific materials.
Globally Harmonized System (GHS) Hazardous Materials Identification System (HMIS) SDS Link
Material Pictograms Signal Word Hazard Statements Health Flammability Hazard Protection
Minspar 200 Health Hazard WARNING May cause damage to lung through prolonged or repeated inhalation 2 0 0 E
Wollastonite (Theoretical) Health Hazard DANGER Vansil W-30 Wollastonite SDS:
May cause cancer if inhaled.
Causes damage to organs through prolonged or repeated exposure if inhaled. (respiratory tract)
EPK HarmfulHealth Hazard DANGER EPK Kaolin is a naturally occurring mineral, which may contain amounts of crystalline silica
typically 0.1-1.0%, may cause damage to respiratory system through prolonged or repeated
exposure.
1 0 0 E
Rutile 1 0 0