Category: Glaze > Yellow
Created 2016-10-07 16:31:27 by William Schran
Categories: Glaze > Yellow
Firing Temperature: Δ10
Atmospheres: Reduction

From William “Bill” Schran, Teacher & Consultant
Creative Creek Artisans: http://www.creativecreekartisans.com/
Cone 10 Reduction Glazes: http://www.creativecreekartisans.com/creativecreek_cone10re.htm

Material Amount Batch Subtotal
Soda Feldspar (Theoretical) 43
EPK 21
Dolomite 14
Whiting 9
Bone Ash 7
Tin Oxide 4
Bentonite 2
Total Base:100
Red iron oxide 0.5
Total: 100.5

Percentage Analysis

Ingredient Amount SiO2 Al2O3 MgO CaO K2O Na2O KNaO P2O5 Fe2O3 TiO2 SnO2 LOI
Soda Feldspar (Theoretical)4329.568.365.085.08
EPK219.67.850.020.040.070.010.080.050.160.083.11
Dolomite143.074.276.67
Whiting95.053.95
Bone Ash73.912.970.13
Tin Oxide44
Bentonite21.190.40.040.020.020.060.080.070.2
Red iron oxide0.50.480.03
Total100.540.3516.613.1313.280.095.165.253.020.710.08414.08
100% no LOI 46.6919.223.6215.370.115.976.073.50.820.094.63

Unity Molecular Formula (UMF)

FLUXES

RO/R2O

0.21 Na2O
0.59 CaO
0.19 MgO
STABILIZERS

R2O3

0.41 Al2O3
GLASS-FORMERS

RO2

1.68 SiO2
0.07 SnO2
OTHER

 

0.01 Fe2O3
0.02 FeO
0.05 P2O5
0.07 CoO
0.02 CuO
SILICA:ALUMINA

SiO2:Al2O3

4.12

FLUX RATIO

R2O:RO

0.21 : 0.79

SiO2:Al2O3 Chart

Closest 100 neighbors in Glaze > Yellow.

Click and drag to zoom
Stull Chart
SiO2:Al2O3 Ratio
SiO2:Al2O3 Ratio 4.12

Similar Base Recipes

No recipes with similar base ingredients and amounts were found.

Similar RO/R2O Unity Formulas

R2O3 - STABILIZERS RO2 - GLASS FORMERS RO/R2O - FLUXES
Recipe Name ΔTemp Al2O3 B2O3 SiO2 ZrO2 SnO2 TiO2 KNaO K2O Na2O CaO MgO ZnO BaO PbO Li2O SrO
Autumn Yellow 10 0.41 1.68 0.07 0.21 0.21 0.59 0.19
Fairbanks' Stony Matt Glaze 9 0.41 1.67 0.07 0.2 0.15 0.05 0.6 0.2

No reviews yet.

Hazards

09/2016 Note: This is a new feature. If a recipe material is not listed, that material's data has not yet been added. Some materials only have GHS ratings, while others only have HMIS ratings. Warnings differ between systems and countries. Glazy does not take any responsibility for accuracy of linked SDS information. Contact your ceramics supplier for safety information for your specific materials.
Globally Harmonized System (GHS) Hazardous Materials Identification System (HMIS) SDS Link
Material Pictograms Signal Word Hazard Statements Health Flammability Hazard Protection
EPK HarmfulHealth Hazard DANGER EPK Kaolin is a naturally occurring mineral, which may contain amounts of crystalline silica
typically 0.1-1.0%, may cause damage to respiratory system through prolonged or repeated
exposure.
1 0 0 E
Dolomite Health Hazard DANGER May cause cancer (Inhalation) 1 0 0 E
Whiting Harmful WARNING Causes eye irritation
Bone Ash
Tin Oxide Harmful WARNING Harmful if swallowed.
Bentonite Harmful WARNING Causes eye irritation
Causes skin irritation
May cause respiratory irritation
Red iron oxide Health Hazard WARNING May cause damage to lung through prolonged or repeated exposure by inhalation