Category: Glaze > Shino > Carbon Trap
Created 2016-10-31 21:56:55 by Adam Yungbluth
Categories: Glaze > Shino > Carbon Trap
Firing Temperature: Δ9-13
Atmospheres: Reduction, Wood

Material Amount Batch Subtotal
Nepheline Syenite (Theoretical) 70
Spodumene (Theoretical) 10
XX Sagger Ball Clay 10
EPK 10
Total Base:100
Soda Ash 8
Total: 108

Percentage Analysis

Ingredient Amount SiO2 Al2O3 MgO CaO Li2O K2O Na2O KNaO P2O5 Fe2O3 TiO2 LOI
Nepheline Syenite (Theoretical)7042.4916.310.070.493.226.8610.080.070.49
Spodumene (Theoretical)106.462.740.8
XX Sagger Ball Clay105.672.920.030.050.090.030.120.070.170.97
EPK104.573.740.010.020.030.010.040.030.080.041.48
Soda Ash8444
Total10859.1925.70.110.560.83.3410.914.240.030.210.216.94
100% no LOI 58.5825.430.110.550.793.3110.7814.090.030.210.21

Unity Molecular Formula (UMF)

FLUXES

RO/R2O

0.7 Na2O
0.14 K2O
0.11 Li2O
0.04 CaO
0.01 MgO
STABILIZERS

R2O3

1.01 Al2O3
GLASS-FORMERS

RO2

3.93 SiO2
0.01 TiO2
OTHER

 

0.01 Fe2O3
SILICA:ALUMINA

SiO2:Al2O3

3.91

FLUX RATIO

R2O:RO

0.95 : 0.05

SiO2:Al2O3 Chart

Closest 20 neighbors in Glaze > Shino > Carbon Trap.

Click and drag to zoom
Stull Chart
SiO2:Al2O3 Ratio
SiO2:Al2O3 Ratio 3.91

Similar Base Recipes

No recipes with similar base ingredients and amounts were found.

Similar RO/R2O Unity Formulas

No recipes with similar RO/R2O Unity Formulas were found.

No reviews yet.

Hazards

09/2016 Note: This is a new feature. If a recipe material is not listed, that material's data has not yet been added. Some materials only have GHS ratings, while others only have HMIS ratings. Warnings differ between systems and countries. Glazy does not take any responsibility for accuracy of linked SDS information. Contact your ceramics supplier for safety information for your specific materials.
Globally Harmonized System (GHS) Hazardous Materials Identification System (HMIS) SDS Link
Material Pictograms Signal Word Hazard Statements Health Flammability Hazard Protection
Spodumene (Theoretical) Health Hazard DANGER May cause cancer by inhalation.
Causes damage to organs through prolonged or repeated exposure.
XX Sagger Ball Clay Health Hazard WARNING May cause damage to lung through prolonged or repeated inhalation. 2 0 0 E
EPK HarmfulHealth Hazard DANGER EPK Kaolin is a naturally occurring mineral, which may contain amounts of crystalline silica
typically 0.1-1.0%, may cause damage to respiratory system through prolonged or repeated
exposure.
1 0 0 E
Soda Ash Harmful WARNING Causes skin irritation.
Causes serious eye irritation.
2 0 0 B