Revised by Virginia Pates - substitute strontium for barium

Material Amount Batch Subtotal
Silica 33.97
Nepheline Syenite (Theoretical) 26.3
Strontium Carbonate 18.9
Lithium Carbonate 14.25
Whiting 3.29
Tennessee ball clay 3.29
Total Base:100
Bentonite 3
Chrome Oxide 0.5
Total: 103.5

Percentage Analysis

Ingredient Amount SiO2 Al2O3 MgO CaO SrO Li2O K2O Na2O KNaO Fe2O3 TiO2 Cr2O3 LOI
Silica33.9733.97
Nepheline Syenite (Theoretical)26.315.966.130.030.181.212.583.790.030.18
Strontium Carbonate18.913.275.63
Lithium Carbonate14.255.818.44
Whiting3.291.851.44
Tennessee ball clay3.291.780.990.010.020.010.010.020.040.050.38
Bentonite31.780.60.060.030.030.090.120.110.3
Chrome Oxide0.50.5
Total103.553.57.720.12.0813.275.811.252.683.930.170.050.516.38
100% no LOI 61.418.860.112.3815.236.661.443.074.510.190.060.57

Unity Molecular Formula (UMF)

FLUXES

RO/R2O

0.1 Na2O
0.03 K2O
0.46 Li2O
0.31 SrO
0.09 CaO
0.01 MgO
STABILIZERS

R2O3

0.18 Al2O3
GLASS-FORMERS

RO2

2.13 SiO2
OTHER

 

0.01 Cr2O3
SILICA:ALUMINA

SiO2:Al2O3

11.76

FLUX RATIO

R2O:RO

0.6 : 0.4

SiO2:Al2O3 Chart

Closest 100 neighbors in Glaze.

Click and drag to zoom
Stull Chart
SiO2:Al2O3 Ratio
SiO2:Al2O3 Ratio 11.76

Similar Base Recipes

No recipes with similar base ingredients and amounts were found.

Similar RO/R2O Unity Formulas

No recipes with similar RO/R2O Unity Formulas were found.

No reviews yet.

Hazards

09/2016 Note: This is a new feature. If a recipe material is not listed, that material's data has not yet been added. Some materials only have GHS ratings, while others only have HMIS ratings. Warnings differ between systems and countries. Glazy does not take any responsibility for accuracy of linked SDS information. Contact your ceramics supplier for safety information for your specific materials.
Globally Harmonized System (GHS) Hazardous Materials Identification System (HMIS) SDS Link
Material Pictograms Signal Word Hazard Statements Health Flammability Hazard Protection
Silica HarmfulHealth Hazard DANGER From 200-Mesh SDS:
May cause cancer by inhalation.
Causes damage to lungs through prolonged or repeated exposure by inhalation.
* 0 0 E
Strontium Carbonate Harmful WARNING Product dust may be irritating to eyes,skin and respiratory system.  1 0 0 E
Lithium Carbonate Harmful WARNING Harmful if swallowed.
Causes serious eye irritation.
Harmful to aquatic life.
Whiting Harmful WARNING Causes eye irritation
Tennessee ball clay Health Hazard WARNING May cause damage to lung through prolonged or repeated inhalation 2 0 0 E
Bentonite Harmful WARNING Causes eye irritation
Causes skin irritation
May cause respiratory irritation
Chrome Oxide WARNING May be harmful if inhaled. May cause
irritation to eyes and respiratory tract. Slightly toxic if ingested.
2 0 1 E