Category: Glaze > Iron
Created 2016-11-10 19:36:09 by Ginger Lukas
Categories: Glaze > Iron
Firing Temperature: Δ6
Atmospheres: Oxidation
Surface Type: Glossy
Transparency: Translucent

Stable lithium base.

Material Amount Batch Subtotal
Silica 55
EPK 20.8
Whiting 16.2
Lithium Carbonate 8
Total Base:100
Red iron oxide 1
Total: 101

Percentage Analysis

Ingredient Amount SiO2 Al2O3 MgO CaO Li2O K2O Na2O KNaO P2O5 Fe2O3 TiO2 LOI
Silica5555
EPK20.89.517.770.020.040.070.010.080.050.160.083.08
Whiting16.29.097.11
Lithium Carbonate83.264.74
Red iron oxide10.950.05
Total10164.517.770.029.133.260.070.010.090.051.110.0814.98
100% no LOI 759.030.0310.613.790.080.020.10.061.290.09

Unity Molecular Formula (UMF)

FLUXES

RO/R2O

0.4 Li2O
0.6 CaO
STABILIZERS

R2O3

0.28 Al2O3
GLASS-FORMERS

RO2

3.93 SiO2
OTHER

 

0.03 Fe2O3
SILICA:ALUMINA

SiO2:Al2O3

14.09

FLUX RATIO

R2O:RO

0.4 : 0.6

SiO2:Al2O3 Chart

Closest 100 neighbors in Glaze > Iron.

Click and drag to zoom
Stull Chart
SiO2:Al2O3 Ratio
SiO2:Al2O3 Ratio 14.09

Similar Base Recipes

Similar RO/R2O Unity Formulas

R2O3 - STABILIZERS RO2 - GLASS FORMERS RO/R2O - FLUXES
Recipe Name ΔTemp Al2O3 B2O3 SiO2 ZrO2 SnO2 TiO2 KNaO K2O Na2O CaO MgO ZnO BaO PbO Li2O SrO
Lithium Clear 6 0.28 3.93 0.6 0.4
Lithium Clear 5-6 0.3 3.98 0.6 0.4

No reviews yet.

Hazards

09/2016 Note: This is a new feature. If a recipe material is not listed, that material's data has not yet been added. Some materials only have GHS ratings, while others only have HMIS ratings. Warnings differ between systems and countries. Glazy does not take any responsibility for accuracy of linked SDS information. Contact your ceramics supplier for safety information for your specific materials.
Globally Harmonized System (GHS) Hazardous Materials Identification System (HMIS) SDS Link
Material Pictograms Signal Word Hazard Statements Health Flammability Hazard Protection
Silica HarmfulHealth Hazard DANGER From 200-Mesh SDS:
May cause cancer by inhalation.
Causes damage to lungs through prolonged or repeated exposure by inhalation.
* 0 0 E
EPK HarmfulHealth Hazard DANGER EPK Kaolin is a naturally occurring mineral, which may contain amounts of crystalline silica
typically 0.1-1.0%, may cause damage to respiratory system through prolonged or repeated
exposure.
1 0 0 E
Whiting Harmful WARNING Causes eye irritation
Lithium Carbonate Harmful WARNING Harmful if swallowed.
Causes serious eye irritation.
Harmful to aquatic life.
Red iron oxide Health Hazard WARNING May cause damage to lung through prolonged or repeated exposure by inhalation