Category: Glaze > Shino
Created 1996-06-03 09:00:00 by Glazy Admin
Categories: Glaze > Shino
Firing Temperature: Δ9-10
Atmospheres: Reduction
Surface Type: Glossy

Glaze Type: Na Li Al Shino

Iron and Rutile are the only colorants that do much for shino type
glazes. Carbon trap glaze. Orange according to the amt. of redtn.
Rust where thin, greys where carbon trapped. For a crawling shino,
sub EPK for calcined kaolin and apply thickly. Glaze Type: Na Li Al
Shino. Opacity: Opaque. Firing type: Reduction From Val Cushing. VC ed

Material Amount Batch Subtotal
Nepheline Syenite (Theoretical) 45
Spodumene (Theoretical) 15
Ball Clay (Theoretical) 15
Kona F-4 feldspar 11
Calcined Kaolin 10
Soda Ash 4
Total Base:100
Bentonite 1
Total: 101

Percentage Analysis

Ingredient Amount SiO2 Al2O3 MgO CaO Li2O K2O Na2O KNaO Fe2O3 TiO2 LOI
Nepheline Syenite (Theoretical)4527.3210.480.050.312.074.416.480.040.32
Spodumene (Theoretical)159.694.111.2
Ball Clay (Theoretical)158.863.750.040.050.140.060.20.150.151.8
Kona F-4 feldspar117.342.150.010.190.530.761.290.02
Calcined Kaolin105.414.59
Soda Ash4222
Bentonite10.590.20.020.010.010.030.040.040.1
Total10159.2125.290.120.561.22.747.26100.240.154.24
100% no LOI 61.1926.140.120.581.242.847.510.340.240.15

Unity Molecular Formula (UMF)

FLUXES

RO/R2O

0.59 Na2O
0.15 K2O
0.2 Li2O
0.05 CaO
0.01 MgO
STABILIZERS

R2O3

1.25 Al2O3
GLASS-FORMERS

RO2

4.95 SiO2
0.01 TiO2
OTHER

 

0.01 Fe2O3
SILICA:ALUMINA

SiO2:Al2O3

3.97

FLUX RATIO

R2O:RO

0.94 : 0.06

SiO2:Al2O3 Chart

Closest 100 neighbors in Glaze > Shino.

Click and drag to zoom
Stull Chart
SiO2:Al2O3 Ratio
SiO2:Al2O3 Ratio 3.97

Similar Base Recipes

No recipes with similar base ingredients and amounts were found.

Similar RO/R2O Unity Formulas

R2O3 - STABILIZERS RO2 - GLASS FORMERS RO/R2O - FLUXES
Recipe Name ΔTemp Al2O3 B2O3 SiO2 ZrO2 SnO2 TiO2 KNaO K2O Na2O CaO MgO ZnO BaO PbO Li2O SrO
Val Cushing Shino Gustin Rev. 9-10 1.25 4.95 0.01 0.74 0.15 0.59 0.05 0.01 0.2
Shino Gustin's #1 9-10 1.2 4.91 0.01 0.74 0.12 0.62 0.04 0.02 0.2
Shino Oestreich #2 9-10 1.3 4.93 0.02 0.74 0.15 0.59 0.05 0.02 0.2
Shino #2 Oestreich 9-10 1.3 4.96 0.01 0.73 0.15 0.58 0.05 0.02 0.2
Shino Orange 9-10 1.2 4.96 0.01 0.73 0.15 0.58 0.05 0.02 0.2

No reviews yet.

Hazards

09/2016 Note: This is a new feature. If a recipe material is not listed, that material's data has not yet been added. Some materials only have GHS ratings, while others only have HMIS ratings. Warnings differ between systems and countries. Glazy does not take any responsibility for accuracy of linked SDS information. Contact your ceramics supplier for safety information for your specific materials.
Globally Harmonized System (GHS) Hazardous Materials Identification System (HMIS) SDS Link
Material Pictograms Signal Word Hazard Statements Health Flammability Hazard Protection
Spodumene (Theoretical) Health Hazard DANGER May cause cancer by inhalation.
Causes damage to organs through prolonged or repeated exposure.
Soda Ash Harmful WARNING Causes skin irritation.
Causes serious eye irritation.
2 0 0 B
Bentonite Harmful WARNING Causes eye irritation
Causes skin irritation
May cause respiratory irritation