Category: Glaze > Shino
Created 2016-12-26 16:36:00 by Anglian Potters
Categories: Glaze > Shino
Firing Temperature: Δ9-11
Atmospheres: Reduction, Salt & Soda, Wood
Surface Type: Satin
Transparency: Opaque

Has previously been used at the annual potters camp on members pots in the salt, soda and wood kilns. test photo is from the wood firing

Material Amount Batch Subtotal
Nepheline Syenite Norwegian 33
Soda Feldspar (Theoretical) 33
Hymod AT Ball Clay 23
Red clay 10
Total: 99

Percentage Analysis

Ingredient Amount SiO2 Al2O3 MgO CaO K2O Na2O KNaO P2O5 Fe2O3 TiO2 LOI
Nepheline Syenite Norwegian3319.37.652.832.55.330.070.66
Soda Feldspar (Theoretical)3322.686.423.93.9
Hymod AT Ball Clay2312.136.50.090.071.010.111.120.520.272.3
Red clay106.51.550.160.030.420.040.460.020.710.110.48
Total9960.622.120.250.094.266.5510.80.021.290.383.44
100%61.2122.350.250.094.36.6110.910.021.310.383.47
100% no LOI 63.4223.150.260.14.456.8511.30.021.350.4

Unity Molecular Formula (UMF)

FLUXES

RO/R2O

0.67 Na2O
0.28 K2O
0.01 CaO
0.04 MgO
STABILIZERS

R2O3

1.37 Al2O3
GLASS-FORMERS

RO2

6.36 SiO2
0.03 TiO2
OTHER

 

0.05 Fe2O3
SILICA:ALUMINA

SiO2:Al2O3

4.65

FLUX RATIO

R2O:RO

0.95 : 0.05

SiO2:Al2O3 Chart

Closest 100 neighbors in Glaze > Shino.

Click and drag to zoom
Stull Chart
SiO2:Al2O3 Ratio
SiO2:Al2O3 Ratio 4.65

Similar Base Recipes

No recipes with similar base ingredients and amounts were found.

Similar RO/R2O Unity Formulas

R2O3 - STABILIZERS RO2 - GLASS FORMERS RO/R2O - FLUXES
Recipe Name ΔTemp Al2O3 B2O3 SiO2 ZrO2 SnO2 TiO2 KNaO K2O Na2O CaO MgO ZnO BaO PbO Li2O SrO
SA Orange Shino 9-11 1.37 6.36 0.03 0.95 0.28 0.67 0.01 0.04
Shino D 9-10 1.36 6.39 0.04 0.97 0.43 0.54 0.02
Ceramic Recipes 2017-08-28 16:04:30
Cone range?

Hazards

09/2016 Note: This is a new feature. If a recipe material is not listed, that material's data has not yet been added. Some materials only have GHS ratings, while others only have HMIS ratings. Warnings differ between systems and countries. Glazy does not take any responsibility for accuracy of linked SDS information. Contact your ceramics supplier for safety information for your specific materials.
Globally Harmonized System (GHS) Hazardous Materials Identification System (HMIS) SDS Link
Material Pictograms Signal Word Hazard Statements Health Flammability Hazard Protection