Category: Glaze > Green > Oribe
Created 2017-01-25 03:34:40 by Clara Giorello
Categories: Glaze > Green > Oribe
Firing Temperature: Δ5-6
Atmospheres: Oxidation
Surface Type: Glossy
Transparency: Transparent

Material Amount Batch Subtotal
Nepheline Syenite (Theoretical) 56.3
Silica 20.8
Frit 3134 12.5
Whiting 10.4
Total Base:100
Copper Carbonate 5
Bentonite 2
Total: 107

Percentage Analysis

Ingredient Amount SiO2 Al2O3 B2O3 MgO CaO K2O Na2O KNaO Fe2O3 CuO LOI
Nepheline Syenite (Theoretical)56.334.1713.120.060.392.595.528.110.060.39
Silica20.820.8
Frit 313412.55.812.892.521.281.28
Whiting10.45.834.57
Copper Carbonate53.221.78
Bentonite21.190.40.040.020.020.060.080.070.2
Total10761.9713.522.890.18.762.616.869.470.133.226.94
100% no LOI 61.9413.512.880.18.762.616.869.470.133.22

Unity Molecular Formula (UMF)

FLUXES

RO/R2O

0.37 Na2O
0.09 K2O
0.53 CaO
0.01 MgO
STABILIZERS

R2O3

0.45 Al2O3
0.14 B2O3
GLASS-FORMERS

RO2

3.47 SiO2
OTHER

 

0.14 CuO
SILICA:ALUMINA

SiO2:Al2O3

7.78

FLUX RATIO

R2O:RO

0.47 : 0.53

SiO2:Al2O3 Chart

Closest 22 neighbors in Glaze > Green > Oribe.

Click and drag to zoom
Stull Chart
SiO2:Al2O3 Ratio
SiO2:Al2O3 Ratio 7.78

Similar RO/R2O Unity Formulas

R2O3 - STABILIZERS RO2 - GLASS FORMERS RO/R2O - FLUXES
Recipe Name ΔTemp Al2O3 B2O3 SiO2 ZrO2 SnO2 TiO2 KNaO K2O Na2O CaO MgO ZnO BaO PbO Li2O SrO
Selsor Oribe (Nephi) 5-6 0.45 0.14 3.47 0.46 0.09 0.37 0.53 0.01
Copper Red Pete's Cranberry 10 0.45 0.14 3.42 0.02 0.43 0.28 0.15 0.53 0.03
Pete's Red 9-12 0.45 0.14 3.43 0.02 0.43 0.28 0.15 0.53 0.03
Selsor Red 5 0.45 0.14 3.47 0.03 0.46 0.09 0.37 0.53 0.01
Selsor Red + Silicon Carbide 6 0.45 0.14 3.47 0.03 0.46 0.09 0.37 0.53 0.01
Selsor Base (Nephi) 5-6 0.45 0.14 3.47 0.46 0.09 0.37 0.53 0.01
Selsor Oribe 2 (Nephi) 5-6 0.45 0.14 3.47 0.46 0.09 0.37 0.53 0.01
Selsor Olive (Nephi) 5-6 0.45 0.14 3.47 0.46 0.09 0.37 0.53 0.01
Selsor Green (Nephi) 5-6 0.45 0.14 3.47 0.46 0.09 0.37 0.53 0.01
Cranbery Red Revised 1 10 0.46 0.16 3.52 0.03 0.43 0.3 0.13 0.57

No reviews yet.

Hazards

09/2016 Note: This is a new feature. If a recipe material is not listed, that material's data has not yet been added. Some materials only have GHS ratings, while others only have HMIS ratings. Warnings differ between systems and countries. Glazy does not take any responsibility for accuracy of linked SDS information. Contact your ceramics supplier for safety information for your specific materials.
Globally Harmonized System (GHS) Hazardous Materials Identification System (HMIS) SDS Link
Material Pictograms Signal Word Hazard Statements Health Flammability Hazard Protection
Silica HarmfulHealth Hazard DANGER From 200-Mesh SDS:
May cause cancer by inhalation.
Causes damage to lungs through prolonged or repeated exposure by inhalation.
* 0 0 E
Whiting Harmful WARNING Causes eye irritation
Copper Carbonate Harmful WARNING Harmful if swallowed.
Causes skin irritation.
Causes serious eye irritation.
Bentonite Harmful WARNING Causes eye irritation
Causes skin irritation
May cause respiratory irritation