Category: Glaze
Created 2017-02-05 07:22:08 by Alisa Liskin Clausen
Categories: Glaze
Firing Temperature: Δ6
Atmospheres: Oxidation
Surface Type: Glossy
Transparency: Translucent

Material Amount Batch Subtotal
Frit 3134 28.6
EPK 28.6
Custer Feldspar 14.3
Silica 14.3
Talc (Theoretical) 7.1
Whiting 7.1
Total Base:100
Mason stain 10
Total: 110

Percentage Analysis

Ingredient Amount SiO2 Al2O3 B2O3 MgO CaO K2O Na2O KNaO P2O5 Fe2O3 TiO2 LOI
Frit 313428.613.36.65.762.942.94
EPK28.613.0810.690.030.050.10.020.120.070.220.114.24
Custer Feldspar14.39.82.430.041.430.431.860.010.04
Silica14.314.3
Talc (Theoretical)7.14.52.260.34
Whiting7.13.983.12
Mason stain10
Total11054.9713.126.62.299.841.533.394.920.070.230.117.73
100% no LOI 59.6614.237.172.4910.671.663.685.340.080.250.12

Unity Molecular Formula (UMF)

FLUXES

RO/R2O

0.18 Na2O
0.05 K2O
0.58 CaO
0.19 MgO
STABILIZERS

R2O3

0.42 Al2O3
0.31 B2O3
GLASS-FORMERS

RO2

3.02 SiO2
SILICA:ALUMINA

SiO2:Al2O3

7.11

FLUX RATIO

R2O:RO

0.23 : 0.77

SiO2:Al2O3 Chart

Closest 100 neighbors in Glaze.

Click and drag to zoom
Stull Chart
SiO2:Al2O3 Ratio
SiO2:Al2O3 Ratio 7.11

Similar Base Recipes

Similar RO/R2O Unity Formulas

R2O3 - STABILIZERS RO2 - GLASS FORMERS RO/R2O - FLUXES
Recipe Name ΔTemp Al2O3 B2O3 SiO2 ZrO2 SnO2 TiO2 KNaO K2O Na2O CaO MgO ZnO BaO PbO Li2O SrO
Gartside 28 ^6 ox. 10 Pink Stain 6 0.42 0.31 3.02 0.23 0.05 0.18 0.58 0.19
Gartside 28, ^6 ox. 1 Tin, 1 Cobalt Carb. 6 0.43 0.31 2.98 0.02 0.23 0.07 0.16 0.58 0.19
Gartside 28, ^6 ox. 3 Nickle 6 0.42 0.31 3.02 0.23 0.05 0.18 0.58 0.19
Gartside 28 ^6 ox. 10 RIO 6 0.42 0.31 3.02 0.23 0.05 0.18 0.58 0.19
Gartside 28 ^6 ox. 5 RIO 6 0.42 0.31 3.02 0.23 0.05 0.18 0.58 0.19
Gartise 28 ^6 ox. 6 Copper Carb. 6 0.42 0.31 3.02 0.23 0.05 0.18 0.58 0.19
Gartise 28 ^6 ox. 6 Copper Carb. 6 0.42 0.31 3.02 0.23 0.05 0.18 0.58 0.19
Gartside 28, ^6 ox. 3 Cobalt Carb., 5 RIO 6 0.42 0.31 3.02 0.23 0.05 0.18 0.58 0.19
Gartside 28 ^6 ox. 2 Cobalt Carb, 3 RIO 6 0.42 0.31 3.02 0.23 0.05 0.18 0.58 0.19
Gartside 28 ^6 ox. 2 Cobalt Carb. 6 0.42 0.31 3.02 0.23 0.05 0.18 0.58 0.19
Gartside 28, ^6 ox. 1 Co. ox. 6 0.42 0.31 3.02 0.23 0.05 0.18 0.58 0.19
Blue Gartside 28 (+Cobalt) (variation) Reids variation (substitute Custer feldspar for G-200 feldspar) 6 0.42 0.31 3.02 0.23 0.05 0.18 0.58 0.19
Gartside 28 Base, Tenmoku (variation) (Reids version, substituted G-200 feldspar for Custer Feldspar) 6 0.42 0.31 3.02 0.23 0.05 0.18 0.58 0.19

No reviews yet.

Hazards

09/2016 Note: This is a new feature. If a recipe material is not listed, that material's data has not yet been added. Some materials only have GHS ratings, while others only have HMIS ratings. Warnings differ between systems and countries. Glazy does not take any responsibility for accuracy of linked SDS information. Contact your ceramics supplier for safety information for your specific materials.
Globally Harmonized System (GHS) Hazardous Materials Identification System (HMIS) SDS Link
Material Pictograms Signal Word Hazard Statements Health Flammability Hazard Protection
EPK HarmfulHealth Hazard DANGER EPK Kaolin is a naturally occurring mineral, which may contain amounts of crystalline silica
typically 0.1-1.0%, may cause damage to respiratory system through prolonged or repeated
exposure.
1 0 0 E
Custer Feldspar HarmfulHealth Hazard WARNING May cause damage to lungs through prolonged or repeated inhalation.
Suspected of causing cancer through
prolonged or repeated inhalation.
May cause allergy or asthma symptoms or breathing difficulties if inhaled.
May cause skin or eye irritation.
Silica HarmfulHealth Hazard DANGER From 200-Mesh SDS:
May cause cancer by inhalation.
Causes damage to lungs through prolonged or repeated exposure by inhalation.
* 0 0 E
Talc (Theoretical) Harmful WARNING Causes mild skin irritation
Harmful if inhaled
May cause respiratory irritation
1 0 0 E
Whiting Harmful WARNING Causes eye irritation